Different methods of synthesizing poly(glycerol sebacate) (PGS): A review

Bruno GodinhoBruno Godinho1Nuno GamaNuno Gama1Artur Ferreira,
Artur Ferreira1,2*
  • 1CICECO-Aveiro Institute of Materials, University of Aveiro, Aveiro, Portugal
  • 2ESTGA-Águeda School of Technology and Management, Águeda, Portugal

Poly(glycerol sebacate) (PGS) is a biodegradable elastomer that has attracted increasing attention as a potential material for applications in biological tissue engineering. The conventional method of synthesis, first described in 2002, is based on the polycondensation of glycerol and sebacic acid, but it is a time-consuming and energy-intensive process. In recent years, new approaches for producing PGS, PGS blends, and PGS copolymers have been reported to not only reduce the time and energy required to obtain the final material but also to adjust the properties and processability of the PGS-based materials based on the desired applications. This review compiles more than 20 years of PGS synthesis reports, reported inconsistencies, and proposed alternatives to more rapidly produce PGS polymer structures or PGS derivatives with tailor-made properties. Synthesis conditions such as temperature, reaction time, reagent ratio, atmosphere, catalysts, microwave-assisted synthesis, and PGS modifications (urethane and acrylate groups, blends, and copolymers) were revisited to present and discuss the diverse alternatives to produce and adapt PGS.

1 Introduction of poly (glycerol sebacate) (PGS)

Poly(glycerol sebacate) (PGS) is a polyester elastomer conventionally produced through the esterification of glycerol with sebacic acid (Figure 1). It is bioresorbable and biodegradable; moreover, its degradation results in non-toxic products. Since its first report as a biocompatible material in 2002 (Wang et al., 2002), PGS has been a research focus of many groups. However, publications before Wang et al. (2002) by Nagata et al. (1996; 1999) described the synthesis of a PGS film (considered a biodegradable polyester) via polycondensation, which was identified as “Yg10” rather than PGS (Nagata et al., 1996; Nagata et al., 1999). The absence of these terms may explain why they have been somewhat forgotten in the literature. Some review articles erroneously consider Wang et al. (2002) the first report of PGS synthesis (Loh et al., 2015; Halil Murat, 2017; Sha et al., 2021; Vogt et al., 2021; Wu et al., 2021).

FIGURE 1
www.frontiersin.org

FIGURE 1. Schematic of the polycondensation of glycerol and sebacic acid to produce poly(glycerol sebacate) (PGS) and possible structures in the polymer chains. “R” = undefined polymer chain.

Several studies have targeted the comprehension and optimization of PGS synthesis and its properties, which have analyzed numerous variables (Liu et al., 2007a; Liu et al., 2007b; Kossivas et al., 2012; Li et al., 2013a; Li et al., 2013b; Guo et al., 2014; Li et al., 2015; Moorhoff et al., 2015; Conejero-García et al., 2017; Gadomska-Gajadhur et al., 2018; Matyszczak et al., 2020; Perin and Felisberti, 2020; Vilariño-Feltrer et al., 2020; Martín-Cabezuelo et al., 2021a; Martín-Cabezuelo et al., 2021b; Wrzecionek et al., 2021; Ning et al., 2022). In addition to these fundamental studies, PGS has been used as a component of polymer blends (Frydrych et al., 2015a; Tallawi et al., 2016; Salehi et al., 2017; Gultekinoglu et al., 2019; Saudi et al., 2019; Fakhrali et al., 2020; Flaig et al., 2020; Gorgani et al., 2020; Kaya et al., 2020; Stowell et al., 2020; Xuan et al., 2020; Behtaj et al., 2021a; Behtaj et al., 2021b; Fakhari et al., 2021; Hanif et al., 2021; Mokhtari and Zargar Kharazi, 2021; Varshosaz et al., 2021; Zhang et al., 2021; Fakhrali et al., 2022), other composite materials (Redenti et al., 2009; Chen et al., 2010; Liang et al., 2011; Gaharwar et al., 2015; Zhou et al., 2015; Rosenbalm et al., 2016; Souza et al., 2017; Tevlek et al., 2017; Zhang et al., 2017; Chen S et al., 2018; Abudula et al., 2020; Fu et al., 2020a; Aghajan et al., 2020; Sencadas et al., 2020a; Lau et al., 2020; Luginina et al., 2020; Rezk et al., 2020; Ruther et al., 2020; Tallá Ferrer et al., 2020; Touré et al., 2020; Zanjanizadeh Ezazi et al., 2020; Piszko et al., 2021a; Atya et al., 2021; Fakhrali et al., 2021; Rastegar et al., 2021; Talebi et al., 2021; Wang et al., 2021; Davoodi et al., 2022), or chemically modified/integrated in the development of PGS copolymers (Tang et al., 2006; Wu Y et al., 2014; Aydin et al., 2016; Jia et al., 2016; Choi et al., 2017; Tang et al., 2017; Zhao et al., 2017; Wang et al., 2018; Wilson et al., 2018; Lang et al., 2020; Rostamian et al., 2020; Chang and Yeh, 2021; Azerêdo et al., 2022; Ruther et al., 2022). PGS-based polymers have been widely employed in electrospinning to produce fibers (Yi and La Van, 2008; Jeffries et al., 2015; Rai et al., 2015; Tallawi et al., 2015; Hou et al., 2017; Hu et al., 2017; Vogt et al., 2018; Wu H. J. et al., 2019; Saudi et al., 2019; Vogt et al., 2019; Abudula et al., 2020; Apsite et al., 2020; Fakhrali et al., 2020; Flaig et al., 2020; Gorgani et al., 2020; Jafari et al., 2020; Keirouz et al., 2020; Silva et al., 2020; Stowell et al., 2020; Touré et al., 2020; Abazari et al., 2021; Bellani et al., 2021; Fakhari et al., 2021; Flaig et al., 2021; Mokhtari and Zargar Kharazi, 2021; Varshosaz et al., 2021; Zhang et al., 2021; Behtouei et al., 2022; Heydari et al., 2022; Rekabgardan et al., 2022; Saudi et al., 2022) and also studied for 3D printing (Yeh et al., 2016; Yeh et al., 2017; Chen S et al., 2018; Pashneh-Tala et al., 2018; Kazemzadeh Farizhandi et al., 2020; Touré et al., 2020; Tsai et al., 2020; Liu et al., 2021; Ruther et al., 2022).

The major focus of PGS-inspired polymers is the development of scaffold material for biological tissue engineering (Wang et al., 2002; Gao et al., 2006; Gao et al., 2007; Jeong and Hollister, 2010; Kemppainen and Hollister, 2010; Masoumi et al., 2013; Khosravi et al., 2016; Ma et al., 2016; Zhang et al., 2016; Nadim et al., 2017; Hsu et al., 2018; Wu W et al., 2019; Hu et al., 2019; Jiang et al., 2019; Xiao et al., 2019; Abudula et al., 2020; Fu et al., 2020a; Apsite et al., 2020; Fu et al., 2020b; Sencadas et al., 2020b; Jafari et al., 2020; Keirouz et al., 2020; Liang et al., 2020; Martín-Pat et al., 2020; Pashneh-Tala et al., 2020; Xuan et al., 2020; Abazari et al., 2021; Behtaj et al., 2021a; Piszko et al., 2021a; Liu et al., 2021; Rastegar et al., 2021; Ângelo et al., 2021; Chen et al., 2022; Fukunishi et al., 2022; Saudi et al., 2022), although many other purposes have been identified for these materials. PGS-based materials have been investigated as drug delivery systems (Sun et al., 2009; Sun et al., 2013; Yang et al., 2017; Ayati Najafabadi et al., 2018; Desai et al., 2018; Oklu et al., 2018; Zhu et al., 2018; Rezk et al., 2020; Zanjanizadeh Ezazi et al., 2020; Sivanesan et al., 2021; Torabi et al., 2021; Heydari et al., 2022; Mehta et al., 2022), adhesives (Mahdavi et al., 2008; Tevlek et al., 2017; Azerêdo et al., 2022), sealants (Chen et al., 2011), coatings (Kim et al., 2014; Lin et al., 2015; Jiang et al., 2020; Zbinden et al., 2020; Zhang et al., 2020; Martín-Cabezuelo et al., 2021b; Ghafarzadeh et al., 2021), biosorbents (Rostamian et al., 2022), membranes for solvents/water pervaporation (Chang et al., 2021), and components for electronic applications (Chen S et al., 2018; Sencadas et al., 2020a; Kazemzadeh Farizhandi et al., 2020; Zhang et al., 2020; Hanif et al., 2021). Their memory shape properties have also been studied (Cai and Liu, 2007; Wu T et al., 2014; Rosenbalm et al., 2016; Wu et al., 2016; Coativy et al., 2017; Tevlek et al., 2020; Xuan et al., 2020). Several reviews have also compiled the research, developments, and applications of PGS and PGS-based materials (Rai et al., 2012; Loh et al., 2015; Halil Murat, 2017; Valerio et al., 2018; Piszko et al., 2021b; Sha et al., 2021; Vogt et al., 2021; Wu et al., 2021; Zulkifli et al., 2022).

The literature used for the present review was identified through searches of the Scopus, Web of Science, Google Scholar, and ResearchGate databases in the Mendeley® application, which was also used to store the database of identified studies. Additionally, we thank the reviewers who also suggested relevant publications to enrich this review article. The search included the following keywords and phrases: “PGS,” “poly(glycerol sebacate),” “poly(glycerol-co-diacids),” “enzymatic synthesis polyesters,” “glycerol polyesters,” “microwave-assisted polyester synthesis,” “PGS-based materials,” etc.

We did not limit the search to any specific period; thus, this review includes relevant publications from 1996 up to 2022.

This review focused on the different synthesis routes used to produce PGS, including its variables and how they influence the polymer properties. The review begins with the conventional method for PGS synthesis via the polycondensation of glycerol with sebacic acid, followed by polycondensation at higher temperatures and microwave-assisted polycondensation. Next, the review describes enzymatic synthesis and the use of other monomers to obtain PGS. Under each of these topics, efforts were made to ensure that the review followed the chronological order of publications whenever possible. We believe that this chronological organization of the publications allows readers to better understand the origin and evolution of knowledge. The following sections present publications on the use of other catalysts and other monomers to obtain the polymer structure of PGS, cross-linking of PGS by photopolymerization, and urethane bonds. The review ends with the properties of PGS and PGS-based materials, where the degradative behavior of these materials is presented in detail (e.g., in vitro, in vitro enzymatic, and in vivo).

This review consolidates the PGS and PGS-based materials synthesis comprehension in their several variables and routes. Therefore, this is a tribute to the knowledge developed over more than 20 years of research, especially publications from the 1990s that were somewhat overlooked, and that also provided fundamental knowledge on the field of PGS.

2 PGS synthesis

2.1 PGS polycondensation synthesis (conventional method)

Traditional PGS synthesis is an energy-intensive and time-consuming process. However, it is considered an economic material (Li et al., 2013a; Kafouris et al., 2013). The conventional method involves a two-step procedure that incorporates a prepolymerization step to form low molecular weight polymers/oligomers, followed by a curing step to cross-link these products and shape the final material. Both steps are normally performed at around 120–150°C, under an inert atmosphere or vacuum, and without catalysts or solvents. Wang et al. (2002) proposed a procedure to produce PGS; subsequent works suggested changes or small adjustments based on those processes (Table 1).

TABLE 1
www.frontiersin.org

TABLE 1. Synthesis conditions for PGS and PGS-based materials.

Studies on the reaction kinetics have shown that the activation energy decreases with increasing molar ratios of glycerol to sebacic acid, which indicates that the reaction is favored at an equimolar ratio of reactants. The reaction kinetics also increase with increasing temperature, showing classical Arrhenius behavior (Maliger et al., 2013; Matyszczak et al., 2020).

Initially, the kinetic control of the reaction advances with first-order kinetics with respect to the monomer. When a given conversion is achieved, the viscosity of the medium increases by changing the reaction to a diffusion-controlled process, which makes it difficult to transfer mass in the system to continue the reaction (Valerio et al., 2018).

PGS properties can be modified by changing the reaction conditions (time, temperature, or reagent ratios) to produce a wide range of mechanical properties (Table 2). Liu et al. (2007a, 2007b) reported that PGS can be a thermoset (TS)PGS or a thermoplastic (TM)PGS depending on the molecular size of the prepolymer used to obtain cured PGS. This may influence the properties and final degradation rate of PGS. Different molecular weights cause the prepolymers to present different viscosities and reactivities in the curing step, which result in distinct branching degrees on the final products.

TABLE 2
www.frontiersin.org

TABLE 2. Mechanical properties of PGS and PGS-based materials.

Li et al. (2013a) identified inconsistencies in PGS properties among research groups using similar synthesis conditions. For example, Chen et al. (2007) and Jaafar et al. (2010) produced PGS with very different Young’s modulus of 1.2 and 0.12 MPa, respectively, despite identical reported synthesis conditions.

As previously stated, different synthesis conditions produce PGS with different properties. Chen et al. (2011) demonstrated some of these differences among research groups and proposed several explanations. For example, the temperature uniformity inside a vacuum oven is ±1°C at best and is typically ±2.5°C for most ovens (Chen et al., 2011). A difference of 5°C can significantly change the cross-linking kinetics of PGS, according to their experiences. Additionally, glycerol loss is problematic and inevitable. The purging flow rate with inert gas and the capacity of the vacuum pump can greatly affect glycerol loss during synthesis, altering the molar relationship of the reagents. Therefore, different research groups report different results, despite using apparently identical synthesis conditions (Chen et al., 2011).

Li et al. (2013a) confirmed that glycerol evaporation is the major cause of irreproducibility. This problem is aggravated when synthesis is performed at high temperatures. At the level of mechanical properties, Young’s modulus of PGS increases with longer cure duration and higher curing temperatures, while the ultimate strength at break decreased. The authors performed detailed 1H NMR and 13C NMR analyses. The results of the NMR analyses show that secondary hydroxyl groups, responsible for cross-link, reacted more slowly than primary hydroxyl groups. Thus, NMR techniques provided qualitative and semi-quantitative structural information on the synthesized PGS. The different structures of acylglycerides identified in PGS are shown in Figure 1.

Li et al. (2015) also identified glycerol loss as a problem. For example, the molar ratios of glycerol to sebacic acid decreased from 0.80 to 0.75 when the curing temperature increased from 120 to 140°C. The authors proposed the use of the degree of esterification to precisely predict the physical status, mechanical properties, and degradation of PGS. Young’s modulus linearly increased with the degree of esterification. Young’s modulus also increased as the total cure time increased, while the elongation at break decreased. Figure 2 illustrates the relationship between the degree of esterification (%) and the physical appearance of PGS at room temperature according to production time and temperature conditions (Li et al., 2015). Figure 2 shows the five physical states that can be observed at room temperature for the production of PGS at different times and temperatures. PGS starts in a waxy solid state, changing to a viscous liquid (gel state), and finally returning to a solid state.

FIGURE 2
www.frontiersin.org

FIGURE 2. (A) Map showing the relationship between the degree of esterification and the state of the sample. The filled squares represent the time and temperature values for thermal treatment where the measurement of the degree of esterification and the physical state of each sample was examined. (B) Pictures of five samples at ambient temperature: A, brittle opaque wax; B, soft translucent wax; C, viscous translucent liquid; D, soft sticky elastomers; E, non-sticky elastomers. The five large squares with letters on top in (A) represent the thermal treatment conditions for the samples shown in (B). Reproduced from Li et al. (2015).

Kafouris et al. (2013) also focused on understanding PGS synthesis by testing different molar ratios of G:S (glycerol:sebacic acid) to produce PGS (2:1, 2:2, 2:3, 2:4, and 2:5), using three reaction steps at 120°C (Table 1). All prepolymers were low molecular weight oligomers, between dimers and nonamers. They concluded that the properties of PGS elastomers are highly dependent on the composition. For example, PGS 2:3 elastomer was the stiffest, with the lowest degree of swelling and sol fraction, while the PGS 2:5 elastomer was one of the softest, exhibiting the highest degree of swelling and sol fraction. The elastomers with compositions far from stoichiometry were softer due to the lower cross-linking density.

In 2017, Conejero-García et al. (2017) assumed a disruptive approach face to the conventional method. It was the first work without vacuum steps and showed the second-highest Young’s modulus reported in the PGS literature (4.7 MPa). The prepolymerization step was conducted at 130°C under an inert atmosphere for 24 h. The curing step was performed in a forced ventilation oven. The resulting films were transparent, soft, and flexible, and became more yellowish and harder with increasing temperature or curing time. This yellowing may be related to the oxidation of the material due to the normal and ventilated atmosphere. The yellowing of polymeric materials due to oxidation is well known (Allen et al., 2022). PGS cured at low temperatures has more non-cross-linked chains and, thus, rinsing promotes a significant loss of mass. In comparison, curing at high temperatures results in more effective cross-linking. The curing time is also important in cross-linking, with mass losses ranging from 6% to 20% for PGS cured at 130°C/48 h and 130°C/24 h, respectively.

The ratio of reagents also influences the efficiency of cross-linking. Similar to Kafouris et al. (2013), Conejero-García et al. (2017) reported superior cross-link density at closer hydroxyl/carboxylic group equilibrium ratios, leading to more robust PGS.

Gadomska-Gajadhur et al. (2018) proposed an optimization of PGS prepolymer (pPGS) synthesis using the Box–Behnken design based on three variables (temperature, G:S molar ratio, and reaction time). The optimization criteria maximized the degree of esterification of PGS and the conversion of monomers. The optimal conditions resulted in a 2:1 molar ratio synthesis at 150°C for 5 h at reflux with stirring (200 rpm), argon atmosphere, and without a catalyst. The resulting pPGS showed a high conversion of the carboxylic groups (∼89%) and a very high degree of esterification (∼82%). The total process time to obtain pure material suitable for medical and pharmaceutical applications was >50 h (Table 1).

While the influences of temperature, time, and reagent molar ratio have been evaluated intensively, the effects of the atmosphere in the PGS reaction have been relatively neglected until recently.

In 2021, Martín-Cabezuelo et al. (2021a) reported the results of a study that aimed to better understand the effect of inert (argon and nitrogen) and oxidative (oxygen, dry air, and humid air) atmospheres in PGS synthesis. The prepolymerization step was performed at 130°C for 24 h with a 1:1 (G:S) molar ratio and different gases flowing through the reactor. The curing step was performed in an oven with forced ventilation at atmospheric pressure (130°C for 48 h). Synthesis at different atmosphere conditions led to PGS networks with significantly different properties. The prepolymerization step showed great extension when performed under oxidative atmospheres, but in a branched way due to the simultaneous formation of oxidized species that boost the reactivity of secondary hydroxyls from glycerol. In contrast, inert atmospheres (Ar even more than N2) promote linear growth of oligomers and low branching. As a result, the increase in viscosity was more gradual in pPGS obtained under inert atmospheres, so the gel point takes longer. After curing, PGS obtained from pPGS produced under oxidative atmospheres is less elastic and softer (Martín-Cabezuelo et al., 2021a).

2.2 PGS polycondensation synthesis (higher temperature approach)

The conventional method of PGS synthesis requires days to complete. To reduce PGS synthesis time, some research groups have used higher temperatures (≥170°C) (Sun et al., 2013; Guo et al., 2014; Gadomska-Gajadhur et al., 2018; Saudi et al., 2019; Riaz et al., 2022). This strategy is described in this section; some examples are also listed in Table 1.

Before the conventional method and the term “PGS” for this polymer were established, the first polycondensation of glycerol with sebacic acid and the production of PGS film (Yg10) were reported by Nagata et al. (1996 and 1999) The temperatures used for synthesis were extremely high and the researchers also used the two-step methodology. Prepolymerization and curing were performed at 200°C and 230°C, respectively, in both publications (Nagata et al., 1996; Nagata et al., 1999).

In 1996, Nagata et al. (1996) prepared aliphatic polyesters from glycerol and a series of various-length aliphatic dicarboxylic acids and analyzed the effects of the methylene chain length on the structure and physicochemical properties, as well as enzymatic degradation. The PGS film was prepared with various curing times (Table 1), which influenced the degree of reaction (%) and, consequently, the enzymatic degradation rate of the film. The PGS films with the best resistance to enzymatic degradation were produced with 2 h of prepolymerization followed by 2 h or 4 h of curing. At 6 h of curing time, the degree of reaction (%) was lower than that at 4 h. Therefore, 6 h was excessive, resulting in thermal degradation of the polymer (Nagata et al., 1996). This PGS film with 6 h of curing was also less resistant to enzymatic degradation.

In 1999, Nagata et al. (1999) prepared PGS copolymers by progressively replacing sebacic acid with other diacids and evaluated the physicochemical and thermal properties, as well as enzymatic degradation. The PGS film was obtained with 43 min of prepolymerization and 4 h of curing time. This very fast synthesis resulted in a material with 1.96 MPa of tensile strength, Young’s modulus of 6.86 MPa, and 27% elongation. Based on these values, this was the strongest and toughest PGS that we found in the literature.

Sun et al. (2013) were the first to report pPGS synthesis and cure at 170°C, significantly reducing the duration of this process. Furthermore, PGS-curcumin polymer was prepared at 185°C. Guo et al. (2014) also produced pPGS at 180°C in only 3.5 h (Table 1).

Matyszczak et al. (2020) created a kinetic model of the polycondensation of sebacic acid with glycerol based on infrared (IR) spectra during the reactions, which allowed the determination of the parameters of the Arrhenius equation over a wide temperature range (130°C–170°C). The polycondensation reaction was performed in an equimolar ratio of reactants at temperatures of 130°C, 150°C, and 170°C for 5–8 h, without any catalyst and under an argon atmosphere at 200 rpm. The disappearance of the 1410 cm−1 peak generated by the acid and an increasing intensity of the 1185 cm−1 ester peak were observed in the real-time IR measurement of the reactions. The polycondensation kinetics were determined based on changes in the intensity of these IR signals.

Saudi et al. (2019) synthesized pPGS under nitrogen gas at 170°C. Glycerol and sebacic acid were combined in a 1:0.8 (G:S) molar ratio as this ratio is more hydrophilic and suitable for cell adhesion and proliferation than other ratios (Guo et al., 2014). Under these conditions, the authors tested three reaction times (3, 5, and 7 h) and analyzed pPGS by Fourier transforming infrared (FTIR). They observed that, beyond 3 h, the sharp carbonyl peak at 1733 cm−1 shifted to 1691 cm−1 and its intensity increased. The sharp peak observed at 1691 cm−1 was related to carbonyl stretching of the unreacted free sebacic acid. Under these conditions, with increasing reaction time, the ester bonds were broken or degraded and a greater proportion of free sebacic acid remained after prepolymer formation. Based on these observations and compared to FTIR of the conventional pPGS synthesis in other studies, the authors suggested 3 h as the ideal reaction time.

The FTIR observations of Saudi et al. (2019) are contrary to the real-time IR spectra of pPGS synthesis reported by Matyszczak et al. (2020). At 5 h, the IR spectra showed a more intense peak related to ester groups compared to that at 3 h. For similar reaction conditions (only a slight ratio change of G:S, 1:0.8 and 1:1), the progression of reactions differed significantly between these studies (Saudi et al., 2019; Matyszczak et al., 2020).

Riaz et al. (2022) synthesized pPGS, mixing the reagents thoroughly for 15 min to ensure homogeneity, heating the reaction mixture at 180°C for 3 h, under continuous nitrogen flow, for use as an ultrasound contrast agent.

Synthesis by the conventional method can take several days without polymer degradation. At very high temperatures, polymer degradation can occur within hours, as reported by Nagata et al. (1996) and Saudi et al. (2019). These higher temperatures can also lead to a severe loss of glycerol. The temperature increase rate must be slow for the monomers to react, forming small monoglycerides (less volatile than glycerol) before reaching high temperatures. Users of this methodology should select the reaction time with care.

2.3 PGS microwave-assisted synthesis

Microwave-assisted synthesis (MwAS) is a time- and energy-efficient pathway to polycondensation reactions. The production of polyesters using microwaves is a relatively solid technology, with application on a non-laboratory scale. For example, in 2009, the first commercial plant for the mass production of poly(lactic acid) via microwave method was developed in Japan (Aydin et al., 2013).

MwAS significantly increases the esterification reaction rate by generating heat homogeneously in a bulk solution via dipole rotation, in which the polar species (e.g., glycerol and lactic acid) align themselves with a rapidly changing electric field produced by the microwaves such that the reactants can be activated selectively. Microwave irradiation provides heat internally and tends to eliminate the “thermal wall effect.” Hence, the condensed water molecules are evaporated faster in the microwave due to their large dielectric constant, which further enhances the polymerization reaction (Coativy et al., 2016; Lau et al., 2017).

Aydin et al. (2013) reported the first attempt to produce PGS using MwAS. The authors proposed an alternative for the initial prepolymerization step in 3 min instead of days, without purge gas, catalyst, vacuum, and agitation. Curing was performed at 150°C and 5 Torr for different time periods. They achieved a PGS after 3 min of prepolymerization and 16 h of cure with Young’s modulus of 0.50 ± 0.02 MPa, tensile strength of 0.27 ± 0.06 MPa, and an elongation of approximately 180%.

However, this MwAS reaction produced a polymer with a molar ratio different from the initial molar composition (G:S, 1:1 to 0.22:0.78). The process resulted in a severe loss of glycerol due to the reaction temperature during the first prepolymerization step, which resulted in the boiling of glycerol monomers, as well as the higher curing temperatures in the second step. The authors also suggested that, since the boiling point of glycerol is 290°C, the decreased time required for polymerization was caused by extremely high temperatures (Aydin et al., 2013).

Li et al. (2015) also performed a MwAS synthesis for prepolymerization. They demonstrated that 15 min of microwave time was as efficient as the conventional prepolymerization method in a nitrogen atmosphere for 6 h at 130°C. However, this rapid synthesis method causes severe glycerol evaporation, resulting in a large alteration in the ratio of the monomers, leading to a more rigid PGS produced under similar curing conditions compared to the conventional prepolymerization method. The temperature of the mixture in the microwave heating process reached 170°C. The glycerol loss was 63% after 30 min of microwave time. This value was significantly higher than the 5%–10% glycerol loss value for the samples prepolymerized for 24 h in a nitrogen atmosphere at 1 atm at 120–140°C.

The results presented in Figure 3 (evolution of the degree of esterification (DE), mass loss (Δm), glycerol loss values, and prepolymerization time) indicate that the rate of esterification decreases faster after 3 min and show a severe loss of glycerol. Thus, the 3 min time is a trade-off between efficient prepolymerization and severe glycerol loss. The authors reported a PGS with Young’s modulus of 0.25 MPa, tensile strength of 0.25 MPa, and an elongation of approximately 190% for a microwave prepolymerization step lasting 3 min and a 48 h cure at 130°C in a vacuum, with a total loss of glycerol of 60%. The PGS properties are close to those reported by Aydin et al. (2013).

FIGURE 3
www.frontiersin.org

FIGURE 3. Evolution of the degree of esterification (DE), mass loss (Δm), and glycerol loss values with increasing prepolymerization time during microwave heating (Li et al., 2015).

Tevlek et al. (2017) also produced pPGS in a microwave oven for 3 min at 650 W to mix with β-tricalcium phosphate (β-TCP) to create a bone-soft tissue interface. The mechanical properties of this material are shown in Table 2.

Recently, Tevlek et al. (2020) reported equimolar PGS with good elasticity (212.75 ± 37.25% elongation) and 0.09 ± 0.03 MPa (Young’s modulus) produced from microwave prepolymerization (4 min, with 10 s intervals every 1 min), followed by curing in a vacuum oven (150°C, 12 h).

Tevlek et al. (2022) also performed PGS prepolymerization in a microwave reactor (White-Westinghouse, United States) at 650 W without any catalyst or extra chemical material. The process was completed by exposing the reagents to microwaves for a total of five times, at 15 s intervals for 1 min. Curing was performed in a vacuum oven at 150°C and 10 mbar for 10, 12, and 14 h, to assess the impact of various cross-linking times on PGS membranes properties. More time (14 h) led to a PGS elastomer with more cross-link density, better biocompatibility, increased tensile strength, and lower elasticity.

Deniz et al. (2020) used a microwave oven (Samsung, Korea) at 650 W and high/medium settings. An equimolar sample of sebacic acid and glycerol mixture was exposed to five rounds of electromagnetic waves for 1 min each at 10-s intervals in the prepolymerization step.

Lau et al. (2017, 2020) proposed a solvent-based system (toluene) to provide better control of the reaction temperature in a microwave cavity and minimize monomer evaporation. Water was collected to measure the degree of esterification. The authors performed MwAS in a CEM Discover SP system, with the reaction maximum temperature well controlled at 130°C. This type of accuracy is impossible in conventional microwave ovens, similar to those used by Aydin et al. (2013) and Li et al. (2015). The curing step was performed at 120°C in a vacuum oven. MwAS was six times faster than conventional heating (CH). For example, 12 min of heating in MwAS, showed a DE of 66%; a similar value of CH required around 75 min. Furthermore, the results of NMR and MALDI-TOF analyses showed that the pPGS produced by MwAS was more branched than that produced by the conventional method without changing the molar ratio of glycerol and sebacic acid. Figure 4 shows proposed PGS structures by both methods. The microwave radiation interacts strongly with glycerol, leading to the activation of both alcohol groups (primary and secondary), which react more efficiently with sebacic acid compared to that in the CH approach.

FIGURE 4
www.frontiersin.org

FIGURE 4. Proposed images of the possible structures of PGS prepolymerized via microwave and conventional methods. Dashed line: cross-linking. Images inspired by Lau et al. (2017).

The higher branching of the pPGS achieved by MwAS facilitates the formation of a cross-linked PGS in a very short curing time. For example, by reducing the curing time to 2 h, PGS specimens prepared by MwAS (DE = 66.82%) showed faster toughening compared to CH samples (DE = 68.18%). The PGS showed Young’s modulus values between 0.7 and 3.14 MPa and elongation between 60% and 15%, depending on curing time. A longer curing time resulted in higher Young’s modulus value and lower elasticity.

Coativy et al. (2016, 2017) also used a microwave approach to synthesize a modified PGS with stearic acid (a Microwave Synthesis Labstation MicroSYNTH with constant agitation). The reaction was performed at 180°C until the viscosity suddenly increased, resulting in the end of magnetic stirring. Stearic acid was used to limit cross-linking to adjust the original properties of PGS to produce a polymer with a memory shape (Coativy et al., 2017). This modified PGS was blended with PLA to increase its ductility (Coativy et al., 2016). Thermogravimetric analysis was performed on pure reagents and the formed polymer (Figure 5). These results were important to explain the glycerol loss behavior with temperature and gas flow. Glycerol showed two mass losses: a small 1% loss between room temperature and 150°C and a severe loss between 150°C and 220°C. This result highlights that glycerol, which is liquid, can be evaporated at a much lower temperature than its boiling point (290°C, 1 atm).

FIGURE 5
www.frontiersin.org

FIGURE 5. Thermogravimetric analysis: variation in reagent weight and biopolyesters under nitrogen flow with a heating ramp of 10°C/min (Coativy et al., 2016)

In addition to the boiling point, the flash point of a substance is also an important property to consider in evaporation processes. The flash point of glycerol is 160°C (Quispe et al., 2013), which confirms the observations of thermogravimetric analysis for the beginning of glycerol mass loss (Figure 5).

Lee et al. (2018) used a microwave reactor (Biotage® Initiator, Charlotte, NC) to cure PGS. The microwave-cured PGS elastomers were similar to PGS elastomers produced by the conventional polycondensation method. The results showed that the microwave curing of PGS is feasible and eight times faster than the conventional curing process, with a maximum cross-link of PGS using a gradual heating up to 160°C for 3 h.

2.4 PGS enzymatic synthesis

Biosynthesis is an alternative to the conventional chemical process of polyester synthesis. Lipase-catalyzed polymerization has been widely investigated because it allows high catalytic activity and high selectivity at mild reaction conditions (preventing side reactions), without harmful components or metallic traces from inorganic catalysts. Enzymatic polymerization was demonstrated as a new methodology in polymer synthesis. Several reviews have addressed this topic (Kobayashi, 2010; Yang et al., 2011; Yu et al., 2012; Zhang et al., 2013; Zhang et al., 2014), including extensive backgrounds on the lipase-catalyzed synthesis of polyesters from polyols and diacids.

Uyama et al. (1999) and Uyama et al. (2001) reported the lipase-catalyzed regioselective polymerization of divinyl sebacate and triols (glycerol-included). These studies produced acylglyceride products through the polymerization of divinyl sebacate and glycerol using Candida antarctica lipase as the catalyst. The reactions were performed at 60°C for 8 h with different reagent ratios. The obtained products were characterized by NMR and SEC analysis. A polymer yield of 63% was obtained in mass after washing. The main unit achieved was 1,3-diaclyglyceride with a small amount of the branching unit 1,2,3-triaclyglyceride. The reagent ratios greatly affected the microstructure of the polymer (molecular mass and glyceride distribution).

Choi and Yoon (2010) registered a patent for the preparation of a biodegradable polymer using an enzyme catalyst. Different sebacate-based polymers are mentioned, including PGS produced by enzyme B as a catalyst, in toluene medium.

Godinho et al. (2018) reported the successful synthesis of pPGS with Candida antarctica lipase B free (CALB) and lipase B immobilized Novozym 435 (N435) with crude glycerol, a by-product of biodiesel production, and glycerol. An equimolar G:S ratio was used, with the reactions performed at 60°C for 24 h in a t-butanol solvent. The products were characterized by MALDI-ToF-MS and NMR. The acid consumption (titration method) was around 75% for the immobilized enzyme and 68% for the free enzyme after 24 h. After rinsing with water, viscous liquid prepolymers were obtained at room temperature, consistent with the PGS map by Li et al. (2015). The MALDI analysis showed that the crude glycerol is favorable for producing cyclic structures, mainly with N435 as a catalyst. Although a clear explanation for this finding is lacking, it may be related to the interaction of NaCl (present in crude glycerol) with the formed oligomers and the enzyme catalytic center. The enzyme types showed differences in acid consumption, and N435 produced richer prepolymer in the range of longer oligomers. In general, multibranched (oligomer with more than one triglyceride structure) or hyperbranched (no free -OH groups in the oligomer) oligomers were not detected, and the 1,3-diaclyglyceride unit was the predominant structure. All prepolymers were mainly composed of low-mass oligomers (<1000 g mol−1), but tridecamers were also detected (<1600 g mol−1).

Perin and Felisberti (2020) used immobilized CALB to produce PGS in mild reaction conditions and studied the kinetics, chain growth, and branching behavior in different reaction conditions (solvents, temperatures, CALB amount, reagents feed ratio). These findings showed that, during the polycondensation reaction, CALB-catalyzed esterification and acyl migration occurred simultaneously. Thus, the PGS architecture changed from linear to branched throughout the progression of the reaction, with the branching resulting from the simultaneous CALB-catalyzed esterification and acyl migration. The different solvents strongly influenced the chain growth. The reactions performed in acetone, at temperatures ranging from 30°C to 50°C, had a higher molecular weight distribution (>10 kDa) compared to those for tetrahydrofuran, t-butanol, or acetonitrile (<3.5 kDa), under the same conditions. Contrary to the conventional method, the increase in temperature did not necessarily mean a faster reaction and higher molecular weight. In acetone, 40°C performed better than 50°C (Perin and Felisberti, 2020).

Avoiding solvents, some works adopted a hybrid way to produce pPGS using enzymatic synthesis. First, the prepolymerization mixture was heated to 120°C, under N2 protection, to form a homogenous transparent liquid mixture. After a 24 h reaction, the temperature was reduced to 90°C and N435 (around 10%–15% of the mass of the starting reagents) was added. The N2 atmosphere was then removed, and vacuum was applied progressively until the end of the reaction, which could take > 60 h (total time) (Lang et al., 2020; Ning et al., 2022). With these reaction procedures, Lang et al. (2020) produced PGS with Mn, Mw, and Đ values of 3700 g/mol, 63,900 g/mol, and 16.9, respectively, after 71 h.

More recently, Ning et al. (2022) demonstrated that N435 catalysis in bulk leads to higher molecular weight PGS compared to that for the conventional method. They also reached an acid consumption of 82% without the formation of a gel fraction, in equimolar reaction conditions, without solvents, at 90°C. The N435 catalysis restricted the interchain cross-linking relations, preventing the gel fraction products, and offered higher selectivity for the reaction of primary hydroxyl units. The N435-catalyzed synthesis enabled the preparation of PGS with Mn, Mw, and Đ values of 6000 g/mol, 59,400 g/mol, and 10 at 67 h, respectively. The authors also explored the application of non-solvents to enrich PGS in higher molecular weight chains by solvent fractionation, with methanol showing the best results.

The use of enzymatic catalysis avoids glycerol loss and significantly reduces the pPGS synthesis time compared to the conventional method. Enzymatic synthesis allows greater control in obtaining oligomers with a linear structure, leaving cross-linking for the curing step. This may be relevant for PGS modifications with alternative cross-linkers, such as acrylate or isocyanate moieties.

2.5 PGS polymer structure synthesis using other catalysts and reagents

PGS has been synthesized mainly by esterification reactions between glycerol and sebacic acid without catalysts. The previous section described some studies using enzymes as catalysts. Two of these studies replaced sebacic acid with divinyl sebacate (Uyama et al., 1999; Uyama et al., 2001). Several publications reported the use of other monomers and catalysts to obtain PGS structures. This section describes publications that used non-enzymatic catalysis and other monomers for PGS-type structure synthesis.

Organometallic catalysts are widely used in industry and research in the polymers field. Wyatt et al. (2012) used dibutyltin (IV)oxide as a catalyst to produce poly(glycerol-co-diacid)s, where sebacic acid was not selected. However, in a recent work, Wilson et al. (2018) used FASCAT 9100 (butylstannoic acid) catalyst to produce pPGS. After curing, a PGS with a tensile strength of 0.84 MPa was produced. In this work, a block copolymer of PGS with poly(tetramethylene oxide) glycol (PTMO) and a mixture of PGS-b-PTMO with a poly(ester-ether) thermoplastic elastomer (Hytrel 3078) was synthesized, producing a polymer, PGS-b-PTMO–Hytrel 3078, with extreme elasticity (2574% elongation).

Diarylborinic acid catalysts promote the formation of linear polyesters from glycerol. Slavko and Taylor (2017) used organoboron catalysts to produce polymers that were essentially free of branching or cross-linking. Sebacoyl chloride was used instead of sebacic acid, and PGS synthesis was performed in THF solvent at 70°C (Slavko and Taylor, 2017). Using sebacoyl chloride and glycerol as monomers and diarylborinic acids as catalysts, a high fraction of 1,3-diaclyglyceride units was found in NMR analysis (Slavko and Taylor, 2017). These findings demonstrated the production of PGS with an essentially linear structure.

Another alternative to PGS synthesis is the ring-opening reaction of diglycidyl sebacate with sebacic acid. Here, diglycidyl sebacate replaces glycerol. This approach aims to produce a linear PGS backbone. This reaction yielded a well-defined linear structure known as poly(sebacoyl diglyceride) PSeD, suitable for functionalization (You et al., 2010; Chen et al., 2016; Wang et al., 2016).

Wrzecionek et al. (2021) developed a method to obtain linear PGS by catalyst-free polytransesterification using glycerol and dimethyl sebacate (2:1 molar ratio, respectively). The authors fixed the molar ratio of the reactants and varied the time and temperature. The synthesis was optimized to minimize the degree of branching and maximize the molecular weight. The optimal parameters obtained for this process were 160°C and 30 h, which produced PGS with a branching degree of 3.5% and a molecular weight of 1.6 kDa.

2.6 PGS photopolymerization (acrylate cross-linking)

The photopolymerization method has been used to obtain a final polymer by introducing reactive acrylate groups into pPGS to form PGS photocurable materials (Figure 6). This approach makes it possible to produce a wide range of physical properties under mild conditions using ultraviolet (UV) light photopolymerization and to reduce the curing step to a few minutes instead of days as in the traditional thermo-curing process. However, the preparation of these photocurable pPGS can also take a long time in functionalization reactions with acrylate groups (Nijst et al., 2007; Ifkovits et al., 2008; Mahdavi et al., 2008; Wu Y et al., 2014; Yeh et al., 2016; Wang M et al., 2017; Wang L et al., 2017; Hu et al., 2017; Yeh et al., 2017; Pashneh-Tala et al., 2018; Chen J.-Y et al., 2018; Singh et al., 2018; Farr et al., 2020; Kazemzadeh Farizhandi et al., 2020; Liang et al., 2020; Pashneh-Tala et al., 2020).

FIGURE 6
www.frontiersin.org

FIGURE 6. Synthesis schemes for PGS prepolymer and PGS-Methacrylate (PGS-M). Scheme from Pashneh-Tala et al. (2018).

Nijst et al. (2007) synthesized PGS acrylate (PGSA) using acryloyl chloride and a photoinitiator (2,2-dimethoxy-2-phenylacetophenone). The synthesis of pPGS followed the traditional method and then was performed with the addition of acrylate moieties. The UV curing step required only 10 min. The elastomers showed Young’s modulus values of 0.05–1.38 MPa, an ultimate tensile strength of 0.05–0.50 MPa, and an elongation at break of 42–189%, depending on the degree of acrylation. Increasing acrylate led to an increased Young’s modulus and decreased elongation capacity. Photocured PGSA networks showed biocompatibility in vitro as assessed by human primary cell adherence and subsequent proliferation into a confluent monolayer. The copolymerization of poly(ethylene glycol) diacrylate with PGSA was also tested and allowed for additional control of final material properties.

Ifkovits et al. (2008) similarly synthesized PGSA as Nijst et al. (2007), with the same conclusions. In general, Young’s modulus increased with an increasing degree of acrylation. The elongation at break increased with increasing molecular weight for a constant degree of acrylation. In their study, the PGSA mechanical properties were 0.15–30 MPa (Young’s modulus) and 5%–200% (elongation). Not all macromers formed an elastomeric network. High acrylation values led to the formation of a very stiff PGSA with low elastomeric characteristics.

Acrylated and methacrylated PGS are biocompatible materials for use in biological tissue engineering applications. These types of materials have been proposed as aid materials for wound dressing (Mahdavi et al., 2008) and nerve guidance conduits (Hu et al., 2017; Singh et al., 2018).

Mahdavi et al. (2008) developed a synthetic gecko-inspired adhesive tissue in PGSA that may be useful for a range of medical applications, including sealing wounds and replacing sutures/staples.

Methacrylated PGS has been proposed for nerve tissue applications (Hu et al., 2017; Singh et al., 2018). Because pPGS is a difficult material to electrospin into nanofibers, Hu et al. (2017) synthesized PGS-based copolymers with methyl methacrylate (MMA), a more easily processed material. Singh et al. (2018) used PGS methacrylate to produce nerve guidance conduits via stereolithography for peripheral nerve injury repair (Figure 7). The material showed appropriate mechanical properties and supported neuronal and glial cell growth in vitro and in vivo.

FIGURE 7
www.frontiersin.org

FIGURE 7. Methacrylated PGS nerve guidance conduits: the left is compressed to highlight the elastic properties, while the right shows the final 3D-printed product ready for implantation (Singh et al., 2018).

Yeh et al. (2016) reported the extrusion-based 3D printing of PGSA to produce scaffolds with elastic properties. This method showed great potential to originate complex biocompatible elastomeric tissues. In the same line of studies, the authors also developed a norbornene-modified PGS (Nor-PGS) that cross-linked faster under ultraviolet light (<1 min), suitable for extrusion-based 3D printing (Yeh et al., 2016).

Tsai et al. (2020) developed a new type of photocurable and elastomeric hydrogel using Nor-PGS-co-polyethylene glycol (Nor-PGS-co-PEG). The norbornene functional groups allowed hydrogel cross-linking via thiol-norbornene photochemistry. The cross-linking process was rapid in the presence of a photoinitiator and UV light (<3 min). Several properties of this material can be easily fine-tuned by adding different amounts of cross-linker. The Nor-PGS-co-PEG can be processed using electrospinning and 3D printing techniques to generate microfibrous scaffolds and printed structures, respectively. The material showed excellent elongation (around 950%) and good cytocompatibility in in vitro studies. Nor-PGS-co-PEG is a promising elastomer with highly tailorable properties for biomedical applications.

Chen J.-Y et al. (2018) described the tunable mechanical and degradation properties for the selection of biodegradable photocurable polymers that may be useful in 3D printing. The authors produced biodegradable photocurable copolymers by copolymerizing polycaprolactone diacrylate (PCLDA) and/or poly(ethylene glycol) diacrylate (PEGDA) with PGSA to form a polymer network. PCLDA and PEGDA are two common choices used in biomedical research. However, the degradation rates of these polymers in vivo are low, limiting their applications. The formation of several copolymers generated a database with selectable properties. The overall degradation rate was significantly higher than those for pure substances.

The direct use of PGS-based biomaterials in in situ tissue and cell encapsulation applications is limited due to their low water uptake. Therefore, Wu Y et al. (2014) developed injectable photocurable biodegradable hydrogels and microgels based on methacrylate poly(ethylene glycol)-co-poly(glycerol sebacate) copolymers. These gels showed good hydration properties and an easy in situ gelation process by photopolymerization under physiological conditions, thus demonstrating their potential as injectable tissue engineering scaffolds.

Pashneh-Tala et al. (2018) and Pashneh-Tala et al. (2020) developed a photocurable PGS methacrylate (PGS-M) prepolymer by functionalization of secondary hydroxyl groups with methacrylic anhydride and triethylamine as catalyst. The authors used different approaches to define the shape of the final material. The authors filled molds with pPGS-M, applied UV light, and photopolymerized a generic disc shape to be CNC carved, creating different objects from digital designs with excellent manufacturing quality and a highly porous structure (Pashneh-Tala et al., 2020). The DLW-2PP (direct laser writing two-photon polymerization) laser technique to obtain 3D structures (Figure 8) was also used to produce PGS-M objects (Pashneh-Tala et al., 2018).

FIGURE 8
www.frontiersin.org

FIGURE 8. PGS-M 3D structures produced by DLW-2PP. Images collected and adapted from Pashneh-Tala et al. (2018).

Wang M et al. (2017) produced a photo/thermo dual curable polymer based on PGS. The functionalization of PGS with 2-isocyanatoethyl methacrylate (IM) quickly produced a methacrylated PGS (PGS-IM). The PGS-IM was synthesized only by mixing PGS with IM at 80°C for 20 min in DMF solvent and without additional reagents/catalysts. After this process, PGS-IM scaffolds were produced by three curing approaches. The thermo-cured scaffolds used a vacuum oven at 150°C at 1 Torr for 12 h. The photo-cured scaffolds were produced using an Irgacure 2959 and UV light for 10 min. The dual-cured scaffold was produced by consecutively applying the previous two curing approaches. The photo-curing was applied first and then the thermo-curing. The combination of these curing processes provided a further way to modulate the properties of the resultant porous scaffolds. All PGS-IM scaffolds showed good elasticity, biodegradability, and cytocompatibility with L929 fibroblast cells. The cross-linking in PGS-IM comprised both acrylate and urethane bonds.

The next section describes the cross-linking of PGS by urethane bonds.

2.7 PGS urethane cross-linking

The use of isocyanates for pPGS cross-linking is another alternative to avoid the long curing times in the conventional process and to produce PGS-derived polymers with improved properties (Pereira et al., 2013; Li et al., 2015; Frydrych and Chen, 2017; Monem et al., 2022). The reaction between isocyanate and free hydroxyl groups occurs rapidly under mild conditions.

Pereira et al. (2013) produced a PGS urethane (PGSU) biocompatible and mechanically tunable elastomer suitable for encapsulation and controlled drug delivery systems. PGSU was synthesized with hexamethylene diisocyanate (HDI) as the cross-linker and tin (II) 2-ethylhexanoate as the catalyst (Figure 9). Pereira et al. (2013) synthesized PGSU films under two conditions: with solvent and solvent free. The solvent-free approach reduced the quantity of solvent traditionally used in film cast and produced films in <36 h. Pereira et al. (2013) reported a wide range of mechanical properties (Young’s modulus from 0.1 MPa to 20 MPa and elongations >400%) for their PGSU films, replicating the characteristics of some biological tissues. The in vitro assessment of the biodegradation and cytocompatibility demonstrated that the degradation profile depended on the degree of cross-linking. Increasing urethane content resulted in slower degradation rates. The degradation rates for all PGSU derivatives were generally slower than that for PGS. Testing of the cytocompatibility of the PGSU materials in human mesenchymal stem cells showed identical metabolism to cells placed in tissue culture polystyrene (TCP) after 8 days of cell proliferation. The inflammatory reaction in vivo of PGSU was significantly lower than that observed for poly(lactic-co-glycolic acid) (PLGA), a degradable material that has been FDA-approved for internal use.

FIGURE 9
www.frontiersin.org

FIGURE 9. Reaction scheme for PGSU synthesis using HDI as a pre-PGS cross-linker. Scheme inspired by Pereira et al. (2013).

Frydrych and Chen (2017) synthesized three-dimensional biodegradable PGSU scaffolds and films via solvent-based synthesis using HDI, tin (II) 2-ethylhexanoate, and 1,4-dioxane as solvent. The PGSU scaffolds showed good hydrophilic characteristics and high-water absorption abilities. In vitro tests, the PGSU scaffolds demonstrated variable degradation rates and mass losses of 10%–16% and 30%–62%, without and with the presence of lipase enzyme, respectively, after 112 days. The results demonstrated that the degradation kinetics of the PGSU scaffolds depended on the urethane content in the PGSU specimens, in which slower degradation rates were linked to higher urethane group numbers, and vice versa, similar to the findings reported by Pereira et al. (2013).

Frydrych et al. (2015b) produced polyester-based polyurethane (PEU) hydrogels based on PGS and poly(ethylene glycol)s (PEG)s. The hydrogels were thermoresponsive, stretchable, biodegradable, and biocompatible. The hydrogels had a tensile Young’s modulus, ultimate tensile strength, and elongation at break in the range of 0.02–0.20 MPa, 0.05–0.47 MPa, and 426%–623%, respectively. In vitro cell tests showed that some of the hydrogels were suitable for culturing adipose-derived stem cells and dermal fibroblasts. These results showed the versatility of these PEU hydrogels for biomedical and engineering applications.

Wang et al. (2018) synthesized PGSU and urethane-based PEGylated PGS elastomers using HDI, tin (II) 2- ethyl-hexanoate, and pPGS and pPEGS. These mixtures were allowed to react at 55°C with stirring for 5 h and under argon flow for cross-linking. By tailoring the PEG and HDI contents, elastomers were produced with broad ranges of mechanical properties and customized hydrophilicities. The mechanical properties of these elastomers are shown in Table 2. Increasing PEG decreased the water contact angle (WCA) to between 28.6–71.5°. The HDI amount had almost no influence on the hydrophobicity of polymers but influenced Young’s modulus and tensile strength. The degradation rate depended on the urethane content in the elastomers, as reported previously (Pereira et al., 2013; Frydrych and Chen, 2017). These elastomers showed favorable biocompatibility in vitro and mild host response in vivo. The results showed that these elastomers could be easily produced into various shapes and be tailored for diverse applications in biomedical research.

Monem et al. (2022) also synthesized PGSU using HDI, tin (II) 2-ethylhexanoate, and 1,4-dioxane as a solvent. In this study, a series of PGSU nanocomposites were synthesized and characterized to produce desirable elastomeric materials. These nanocomposites were prepared with two kinds of nanoclay under the commercial names of Cloisite Na+ and Cloisite 10 A. The results indicated that both nanoclays enhanced the storage modulus. Hydrolytic degradation of the nanocomposites indicated that the degradation behaviors of the samples were highly affected by their hydrophilicity properties. The neat PGSU showed a mass loss of 63.5 ± 1% after 30 days (degradation rate ∼15% per week) and a WCA close to 80°. The more resistant PGSU nanocomposite to degradation showed a mass loss of 48.9 ± 1% after 30 days (degradation rate ∼11% per week) and a WCA close to 90°.

Golbaten-Mofrad et al. (2021) similarly produced PGSU using HDI, tin (II) 2-ethylhexanoate, and a solvent mixture of DMSO:DMF (70:30 wt%). The solution was stirred at 55°C for 15 min. In this research experiment, a series of PGSU scaffolds with various cross-link densities were prepared for subsequent polypyrrole polymerization and insertion of zinc oxide (ZnO) nanoparticles. The mechanical performance of the scaffolds under dry and hydrated conditions was evaluated by compression tests. Hydrated low urethane content scaffolds presented Young’s modulus and compression stress at 75% strain in the ranges of 8.1–9.4 kPa and 26.6–29.8 kPa, respectively. In contrast, the high urethane content scaffolds displayed higher Young’s modulus values and compression stress at 75% strain in the ranges of 48.8–122.5 kPa and 927.9–1014.5 kPa, respectively. The ZnO nanoparticles improved the surface hydrophilicity (WCA 86°) and added anti-bacterial behavior (WCA 97.2°). The high HDI molar ratio intensified the samples’ surface hydrophobicity (WCA 102.9°).

Li et al. (2015) also synthesized PGSU, but with methylene diphenyl diisocyanate (MDI) as the cross-linker. They observed that MDI resulted in a more rigid polymer compared to PGS. Thus, isocyanate introduction must be moderate because excessive amounts remove the elastomeric properties of the final material.

3 PGS material properties

PGS is presently characterized as a material that resembles soft biological tissues. Its mechanical properties (Table 2) are close to those of some biological tissues, such as the cornea, the arteries/veins, the spinal cord, the gray matter, and some muscles (McKee et al., 2011). Because sebacic acid and glycerol both have endogenous natures, PGS and PGS-based materials are considered to be biocompatible (Piszko et al., 2021b). Moreover, glycerol and sebacic acid have been approved by the FDA; therefore, PGS degradation products are considered safe (Kemppainen and Hollister, 2010; Sha et al., 2021). PGS polyester elastomer can appear as transparent, almost odorless, and colorless or slightly yellow (depending on oxygen present during the reaction) (Halil Murat, 2017; Piszko et al., 2021b). PGS forms a covalently cross-linked 3D network of random coils with hydroxyl groups on the backbone (Sha et al., 2021). The PGS density is around 1.13 g/cm3 (Nagata et al., 1996; Pomerantseva et al., 2009).

pPGS is soluble in many available organic solvents, including 1,3-dioxolane, THF, dimethyl carbonate, ethanol, isopropanol, DMF, dioxane, acetic acid, formic acid, and acetone (Halil Murat, 2017; Piszko et al., 2021b). This makes processing easier and allows the use of a variety of techniques.

The physicochemical properties of PGS are commonly assessed by FTIR and NMR. These analyses are useful for screening the synthesis progress and characterizing the final material. FTIR confirms the presence of all important bonds and functional groups including polar hydroxyl, terminal carboxyl groups, ester bonding, and aliphatic backbone. NMR analysis allows for effective structural characterization of the prepolymer before subsequent cross-linking or modification, as well as analyses of the molecular chain topology (Wyatt et al., 2012; Li et al., 2013a; Halil Murat, 2017; Perin and Felisberti, 2020; Piszko et al., 2021a; Piszko et al., 2021b; Ning et al., 2022).

The thermal stability of PGS, as evaluated by thermal gravimetric analysis (TGA), is consistent throughout the literature. PGS is stable up to 250°C and shows a single weight loss step between 320°C and 475°C (Gaharwar et al., 2015; Tang et al., 2017; Aghajan et al., 2020; Rostamian et al., 2020; Martín-Cabezuelo et al., 2021a; Chang et al., 2021). The initial degradation temperature starts between 320°C and 350°C, with a peak degradation temperature typically between 435°C and 440°C (Gaharwar et al., 2015; Aghajan et al., 2020; Martín-Cabezuelo et al., 2021a; Piszko et al., 2021a). However, Martín-Cabezuelo et al. (2021a) studied the effects of the PGS synthesis under different atmospheres and observed a lower peak of thermal degradation (415°C and 425°C for hydrated and dry air, respectively) when PGS was synthesized using air (Martín-Cabezuelo et al., 2021a).

The thermal properties of PGS, as assessed by differential scanning calorimetry (DSC), are also consistent in the literature. PGS is a semi-crystalline polymer, with properties that depend on the glass transition temperature (Tg) of the amorphous phase and melting temperature (Tm) of the crystalline phase (Cai and Liu, 2007; Jaafar et al., 2010). The degree of crystallization decreases significantly with the extent of cure (Jaafar et al., 2010; Guo et al., 2014). The Tg of PGS ranged between −40°C and −15°C, with a broad melting transition between −20°C and 40°C according to the DSC diagrams (Cai and Liu, 2007; Jaafar et al., 2010; Conejero-García et al., 2017). PGS is completely amorphous >35°C (Cai and Liu, 2007; Jaafar et al., 2010; Rostamian et al., 2020). The dynamic mechanical thermal analysis (DMTA) results are consistent across many publications. The temperature at the maximum of the associated peak in tan δ shifts accordingly to lower temperatures, around -20°C, which characterizes the main relaxation process associated with the Tg of PGS (Aghajan et al., 2020; Rostamian et al., 2020; Martín-Cabezuelo et al., 2021a; Chang et al., 2021).

The crystallinity and morphology of PGS can be assessed by X-ray diffraction (XRD) analysis. PGS shows a broad amorphous peak at about 2θ = 20° which is related to the short-range regular ordered structure of both free and cured chains along with the disordered structure of the amorphous phase of the PGS matrix (Nagata et al., 1996; Nagata et al., 1999; Chen et al., 2007; Guo et al., 2014; Aghajan et al., 2020).

PGS is considered hydrophilic, with a WCA around 38–94° (Guo et al., 2014; Gaharwar et al., 2015; Aghajan et al., 2020; Chang et al., 2021; Martín-Cabezuelo et al., 2021a; Tevlek et al., 2022). A higher glycerol ratio synthesis promotes decreased WCA as it increases the number of hydroxyl groups. However, a higher ratio of sebacic acid increases the hydrophobic group content and WCA values (Guo et al., 2014). For PGS produced from a molar reagent ratio of 1:1 (G:S), the increase in cross-link density, which consumes more hydroxyl groups, provides more wettable surfaces (Conejero-García et al., 2017; Tevlek et al., 2022). However, when the cross-link density increases by urethane (Golbaten-Mofrad et al., 2021) or methacrylate (Singh et al., 2018) bonds, the WCA value increases (Singh et al., 2018; Golbaten-Mofrad et al., 2021). This can be contradictory. However, the hydrophilicity of PGS elastomers is related not only to the presence of hydroxyl groups but also to the polar end groups and inter-molecular hydrogen bonds (Conejero-García et al., 2017; Tevlek et al., 2022). The WCA value of a PGS material is a good indicator of cell viability as more wettable surfaces promote better cell adhesion and propagation (Fakhari et al., 2021; Tevlek et al., 2022).

Based on the ISO 10,993-5 standard, materials with cell viability <70% are considered toxic. PGS can cause cytotoxicity in vitro due to acidic components released into the culture medium because of surface degradation (Li et al., 2013b; Tevlek et al., 2022). PGS elastomers with lower cross-link density degrade faster than those with higher cross-link density, in the same environmental conditions. The unreacted carboxylic acid groups and/or the carboxylic acids produced by the hydrolysis of ester groups can cause severe acidification of the medium (Li et al., 2013b), leading to higher cytotoxicity of PGS elastomers with lower cross-link density (Chen et al., 2011; Li et al., 2013b; Tevlek et al., 2022). Moreover, Liu et al. (2009) reported high cytotoxicity of a PGS elastomer modified with citric acid (PGSC). After 7 days, the accumulated acidity of the acidic sols inhibited the growth of L-929 cells, causing most of the cells to die (Liu et al., 2009). These findings confirmed that excessive acidity caused by elastomer degradation leads to high cytotoxicity levels.

However, the addition of another acid monomer to the polymer structure does not necessarily imply increased cytotoxicity. Chen et al. (2011) reported that the addition of lactic acid to PGS to obtain (PGS-co-LA) significantly improved the cytocompatibility of the final materials compared to the PGS alone.

PGS and PGS-based materials are non-toxic when synthesized properly. The cytocompatibility of PGS has been demonstrated in NIH 3T3 fibroblasts (Wang et al., 2002), 3T3 fibroblasts (Rai et al., 2013a; Jeffries et al., 2015), MC3T3 osteoblasts (Wu et al., 2016), chondrocytes (Wu et al., 2016), human umbilical artery smooth muscle cells (HUASMCs) (You et al., 2016; Hsu et al., 2018; Wu H. J et al., 2019), SNL mouse fibroblasts (Chen et al., 2011; Li et al., 2013b; Xu et al., 2015), L-929 fibroblasts, (Conejero-García et al., 2017; Varshosaz et al., 2021; Wang et al., 2021; Jia et al., 2016; Tang et al., 2017; Wu et al., 2016; Wang M et al., 2017) human umbilical vein endothelial cells (HUVECs) (Wang et al., 2021; Zhang et al., 2021; Tevlek et al., 2022), hFOB1.19 human fetal osteoblasts (cytocompatibility and osteoconductivity) (Piszko et al., 2021a), Schwann cells (Sundback et al., 2005; Singh et al., 2018), bone marrow stromal cells (BMSCs) (Wang et al., 2018), human mesenchymal stem cells (hMSCs) (Pereira et al., 2013), and human dermal fibroblasts (Pashneh-Tala et al., 2020).

PGS and PGS-based material biocompatibility has been demonstrated in vivo in BALB/c adult mice (Piszko et al., 2021a), CD® (Sprague-Dawley) IGS rats (Fu et al., 2020b), Sprague-Dawley rats (Wang et al., 2002; Ifkovits et al., 2008; Jia et al., 2016; Ma et al., 2016; Wu et al., 2016; Xiao et al., 2019), Wistar rats (Mahdavi et al., 2008; Sun et al., 2009), Fisher rats (Sundback et al., 2005), rabbits (osteoconductive to bone regeneration) (Zaky et al., 2017), C57 rats (Wang et al., 2018), YFP+ mice (Singh et al., 2018), and Lewis rats (Pomerantseva et al., 2009; Pereira et al., 2013). In vivo, some mild and temporary inflammatory responses typical of implantable biodegradable polymers have been reported with PGS and PGS-based materials; however, necrosis or tissue degradation have not been reported (Ifkovits et al., 2008; Pomerantseva et al., 2009; Sun et al., 2009; Wu et al., 2016; Fu et al., 2020b).

Table 2 presents the mechanical properties of different PGS-based materials found in the bibliography. The data shows how compliant PGS can be with other elements, allowing the production of new materials with different or improved mechanical properties.

3.1 PGS degradation (in vitro hydrolytic, in vitro enzymatic, and in vivo)

PGS degradation can be evaluated by three methods: in vitro hydrolysis degradation, in vitro enzymatic degradation, and in vivo degradation. Independent of the degradation type, the PGS degradation process follows the surface erosion mechanism (Wang et al., 2003; Sundback et al., 2005; Pomerantseva et al., 2009; Guo et al., 2014; Kim et al., 2014; Li et al., 2015; Souza et al., 2017; Zhang et al., 2020; Tevlek et al., 2022). This mechanism is characterized by linear mass loss and corresponding volume decrease while preserving the shape, surface integrity, and mechanical properties. The surface erosion mechanism has also been observed in many PGS-based materials such as PGSU (Pereira et al., 2013; Frydrych and Chen, 2017), PGS-M (Pashneh-Tala et al., 2018), and other PGS-based materials (Ma et al., 2016; Lang et al., 2020).

However, Shi et al. (2020) demonstrated that induced cracks overcome erosion in PGS and lead to the premature loss of the mechanical properties and morphology of the material. The crack progression depends on pH, humidity, and applied forces (Shi et al., 2020).

The degradation rate, for the same conditions, is related to the cross-link density of PGS materials, in which materials with higher cross-link densities show more resistance to degradation (Pereira et al., 2013; Li et al., 2015; Frydrych and Chen, 2017; Lau et al., 2017; Singh et al., 2018; Krook et al., 2020).

Krook et al. (2020) investigated the degradation of porous PGS, reporting that the polymer properties change rapidly with degradation in the case of materials with lower cross-link density.

3.1.1 In vitro hydrolytic degradation

The in vitro hydrolytic degradation is typically performed in a buffered aqueous solution (pH 7.4), at 37°C under agitation. This type of degradation is the slowest.

One study reported that the PGS samples lost 15%–30% of the mass, depending on the cross-link density, during the 28-day process of hydrolytic degradation (Li et al., 2015). In another study, the PGS slowly degraded, losing only 17% of the mass in 60 days (Sundback et al., 2005).

In another study, PGS-IM scaffolds degraded in vitro showed mass losses of 12.2% (photo-cured), 11.9% (thermo-cured), and 5.9% (dual-cured), respectively, at day 28. The dual-cured scaffolds showed the lowest mass loss rate, likely due to their highest cross-link density (Wang M et al., 2017). Once again, this process of degradation is slower.

3.1.2 In vitro enzymatic degradation

The in vitro enzymatic degradation is usually performed in an aqueous buffered solution (pH 7.4), with enzymes (e.g., lipases and esterases), at 37°C, and under agitation. The use of enzymes accelerates the degradation process.

Nagata et al. (1996) performed the in vitro degradation of PGS films with lipase. After 6 h, a weight loss of 80 g/m2 was observed for PGS films, with a reaction degree of 83%. The degree of reaction affected the degradation. PGS films with higher degrees of reaction showed higher resistance to degradation.

Nagata et al. (1999) performed in vitro degradation of PGS copolymers films with lipase. The films were obtained by incorporating other diacids in the polymer synthesis. The various PGS copolymers films produced were compared after 2 h of enzymatic degradation. The PGS film had a weight loss of 50 g/m2; however, the addition of other diacids increased the resistance of the copolymer films. For example, replacing 10% (mol) of sebacic acid with succinic acid resulted in a PGS-co-succinate film, “Yg-10/4 (90/10)”, which had a weight loss of 22 g/m2, an increase in degradation resistance of >50%, compared to PGS.

Tevlek et al. (2022) cured three sets of PGS elastomers for different times (14, 12, and 10 h) and performed in vitro hydrolytic and enzymatic degradations in a 28-day process. The hydrolytic mass losses were 9.65%, 13.79%, and 24.82%, and the enzymatic degradation mass losses were 12.75%, 19.54%, and 43.75%, respectively. The cross-link densities were 70.33, 33.79, and 14.77 mol/m3, respectively. Their data confirmed that enzymatic degradation was faster than hydrolytic degradation and that the degradation rate of both depended on the cross-link density.

In a 4-day process, Pereira et al. (2013) performed in vitro enzymatic degradation in PGS and PGSU with different degrees of urethane cross-linking. The PGS samples were completely degraded in 4 days, while the mass was progressively lost in the PGSU samples due to their cross-link density. The PGSU samples with the highest cross-link densities showed 0% mass loss (no degradation).

Frydrych and Chen (2017) performed in vitro degradation tests in PGSU scaffolds, which showed adjustable degradation rates and mass losses of 8.7%–16.3% and 10.7%–20.7% without and with the presence of enzyme, respectively, after 31 days. Enzymatic degradation was faster than hydrolytic degradation.

Singh et al. (2018) performed PGS-M hydrolytic degradation studies after 40 days, in which the implants showed no change in mass (no degradation). Enzymatic degradation results indicated a decrease in the degradation rate of the polymer with an increased degree of methacrylation. The results of enzymatic degradation showed a decreased rate of polymer degradation with an increased degree of methacrylation. At the highest methacrylation cross-linking the degradation rate was null (no degradation).

The information presented thus far in this review showed that the modification of PGS can lead to significantly increased resistance to degradation.

3.1.3 In vivo degradation

In vivo degradation is performed by placing the object to degrade inside an animal (e.g., mice or rats). In in vivo trials, the environment is more dynamic, with a more fluid exchange of molecules and removal of any degradation products around the implant. The presence of various enzymes in their natural environment also has a greater impact on degradation, compared to in vitro trials (Ifkovits et al., 2008; Pomerantseva et al., 2009). The in vivo degradation rate of PGS is much faster than the in vitro degradation rate.

Wang et al. (2002) demonstrated the differences between in vitro and the in vivo PGS degradation. In the 60-day trials, the measured in vitro hydrolytic degradation of PGS resulted in a 17.6% mass loss, while PGS implanted in Sprague-Dawley rats were completely consumed in the same time.

Wang et al. (2003) implanted PGS samples subcutaneously in female Sprague-Dawley rats and evaluated them after 35 days. The PGS implants maintained their geometries throughout the time periods. The implants lost weight gradually and linearly over the test period of 35 days, during which time >70% of their mass.

Another study implanted PGS samples in male Fisher rats, after which the degradation was evaluated for 60 days. After 35 days, the geometry of the PGS implants was the same as that on day 1; however, the volume was almost half that measured initially. The implants gradually decreased in size, consistent with a mechanism of surface erosion. After 60 days, the implants were difficult to detect and no dimensional data were obtained (Sundback et al., 2005).

The PGS was almost completely degraded within 14 days in the arterial circulation of Sprague-Dawley IGS rats (Fu et al., 2020a).

Ding et al. (2017) added tyramine (TA) to PGS and placed the PGS-TA and PGS in male BALB/cJ mice. After 14 days, both implants had completely degraded in vivo.

The rapid degradation of PGS may limit its use in tissues that require long-term mechanical support but may be useful for the controlled release of drugs in short-term treatments.

PGS implants loaded with 5-fluorouracil (5-FU-PGS) placed in Wistar rats maintained their geometries and decreased in bulk throughout the degradation period of 30 days. The mass loss in vivo (30%) was much higher than that in vitro (10%). The results of the in vitro anti-tumor activity assay suggested the anti-tumor activity of 5-FU-PGSs exhibited through sustained drug release. These results showed that PGS is a good candidate for drug delivery systems (Sun et al., 2009).

The rapid hydrolysis of PGS limits its application as a scaffold material in tissue engineering applications, particularly when healing is slow (i.e., from months to years) (Lang et al., 2020).

However, PGS showed good results for guided tissue regeneration. Upon implanting PGS in the rabbit ulnar defect, histology and tomography analysis at 8 weeks showed that gap filling with the new bone, guided by the PGS elastomer (Zaky et al., 2017).

Another way to use PGS for long-term treatment is by mixing it with other components.

PGS combined with chondroitinase ABC (ChABC) promoted spinal cord repair in rats in 12 weeks. The combination of PGS and ChABC resulted in augmented nerve regeneration and partial functional recovery, better than PGS or ChABC independently (Pan et al., 2018). A recent study used PGS scaffolds to restore a wounded rat uterus, which promoted BMSC attachment and growth and increased blood vessel regeneration in 90 days (Xiao et al., 2019).

PGS modification by functionalization of the hydroxyl groups with palmitates (palmitate-PGS) has been successfully shown to delay degradation (Fu et al., 2020b; Ding et al., 2020). In vivo tests with CD® (Sprague-Dawley) IGS rats showed that palmitate-PGS degraded over 4–12 weeks compared to only 2 weeks for PGS alone (Fu et al., 2020b).

PGSA samples were implanted in Sprague-Dawley rats. After 4 weeks, the in vivo mass loss (25%) was greater than in vitro hydrolytic (12%). Past 8 weeks, the in vivo mass loss (37%) was nearly the same at the in vitro hydrolytic mass loss (33%) (Ifkovits et al., 2008).

4 Outlook/Conclusion

PGS is an elastomer-type polymer with great potential in the biomedical field because its biocompatibility and properties can be tailored to biological tissues. PGS is typically produced through the polycondensation of glycerol and sebacic acid. However, its synthesis has also been reported using divinyl sebacate or sebacoyl chloride with glycerol. Another alternative method of producing PGS is by ring-opening reaction of diglycidyl sebacate with sebacic acid, which results in a well-defined linear structure known as PSeD.

PGS was mainly produced by the conventional method, which is energy-intensive and time-consuming without the use of solvents or catalysts. One strategy to reduce the reaction time is increasing the temperature to >150°C. However, this option can lead to a significant loss of glycerol and an increased number of branches and/or cross-links in the polymer chain and, thus, a more rigid material.

MwAS reportedly produces pPGS in minutes instead of hours or days and is mainly mixed with other materials. Microwave radiation promotes the growth of undifferentiated polymers, in which the primary and secondary hydroxyl groups have the same reactivity with carboxylic acid groups. This type of pre-PGS is richer in cross-linked structures (triacylglycerides) and requires less time to cure.

The use of catalysts is the least often described approach to potentially reduce reaction time. Enzymes and diarylborinic acids can be used to reduce the reaction time and temperature by promoting linear structures. However, the use of solvents requires polymer separation and purification steps.

Another strategy to reduce the PGS synthesis time is the modification of pPGS with cross-linkers such as isocyanates and acrylates that speed curing. Isocyanates allow fast cross-linking via urethane bonds, while acrylate and methacrylate allow fast cross-linking by photopolymerization.

PGS has been frequently combined with other molecules and polymers to produce materials with more desirable properties. Individually, PGS has a high biodegradability in vivo that is not suitable for long-term applications. However, its biocompatibility and safety are well proven, which makes PGS a valid polymer for the development of materials for biomedical applications.

Author contributions

All authors have made substantial, direct, and intellectual contributions to the work and approved its publication.

Funding

This work was developed within the scope of the project CICECO-Aveiro Institute of Materials (UIDB/50011/2020, UIDP/50011/2020, and LA/P/0006/2020), financed by national funds through the FCT/MEC (PIDDAC).

Conflict of interest

The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Publisher’s note

All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors, and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.

References

Abazari, M. F., Zare Karizi, S., Samadian, H., Nasiri, N., Askari, H., Asghari, M., et al. (2021). Poly (glycerol sebacate) and polyhydroxybutyrate electrospun nanocomposite facilitates osteogenic differentiation of mesenchymal stem cells. J. Drug Deliv. Sci. Technol. 66, 102796. doi:10.1016/j.jddst.2021.102796

CrossRef Full Text | Google Scholar

Abudula, T., Gauthaman, K., Hammad, A., Joshi Navare, K., Alshahrie, A., Bencherif, S., et al. (2020). Oxygen-releasing antibacterial nanofibrous scaffolds for tissue engineering applications. Polym. (Basel) 12, 1233. doi:10.3390/polym12061233

CrossRef Full Text | Google Scholar

Aghajan, M. H., Panahi-Sarmad, M., Alikarami, N., Shojaei, S., Saeidi, A., Khonakdar, H. A., et al. (2020). Using solvent-free approach for preparing innovative biopolymer nanocomposites based on PGS/gelatin. Eur. Polym. J. 131, 109720. doi:10.1016/j.eurpolymj.2020.109720

CrossRef Full Text | Google Scholar

Allen, N. S., Edge, M., and Hussain, S. (2022). Perspectives on yellowing in the degradation of polymer materials: inter-relationship of structure, mechanisms and modes of stabilisation. Polym. Degrad. Stab. 201, 109977. doi:10.1016/j.polymdegradstab.2022.109977

CrossRef Full Text | Google Scholar

Ângelo, D. F., Wang, Y., Morouco, P., Monje, F., Monico, L., Gonzalez-Garcia, R., et al. (2021). A randomized controlled preclinical trial on 3 interposal temporomandibular joint disc implants: TEMPOJIMS—phase 2. J. Tissue Eng. Regen. Med. 15, 852–868. doi:10.1002/term.3230

PubMed Abstract | CrossRef Full Text | Google Scholar

Apsite, I., Constante, G., Dulle, M., Vogt, L., Caspari, A., Boccaccini, A. R., et al. (2020). 4D Biofabrication of fibrous artificial nerve graft for neuron regeneration. Biofabrication 12, 035027. doi:10.1088/1758-5090/ab94cf

PubMed Abstract | CrossRef Full Text | Google Scholar

Atya, A. M. N., Tevlek, A., Almemar, M., Gökcen, D., and Aydin, H. M. (2021). Fabrication and characterization of carbon aerogel/poly(glycerol-sebacate) patches for cardiac tissue engineering. Biomed. Mat. 16, 065027. doi:10.1088/1748-605x/ac2dd3

PubMed Abstract | CrossRef Full Text | Google Scholar

Ayati Najafabadi, S. A., Shirazaki, P., Zargar Kharazi, A., Varshosaz, J., Tahriri, M., and Tayebi, L. (2018). Evaluation of sustained ciprofloxacin release of biodegradable electrospun gelatin/poly(glycerol sebacate) mat membranes for wound dressing applications. Asia. Pac. J. Chem. Eng. 13, e2255. doi:10.1002/apj.2255

CrossRef Full Text | Google Scholar

Aydin, H. M., Salimi, K., Rzayev, Z. M. O., and Pişkin, E. (2013). Microwave-assisted rapid synthesis of poly(glycerol-sebacate) elastomers. Biomater. Sci. 1, 503. doi:10.1039/c3bm00157a

PubMed Abstract | CrossRef Full Text | Google Scholar

Aydin, H. M., Salimi, K., Yilmaz, M., Turk, M., Rzayev, Z. M. O., and Piskin, E. (2016). Synthesis and characterization of poly(glycerol-co-sebacate-co-ε-caprolactone) elastomers. J. Tissue Eng. Regen. Med. 10, E14–E22. doi:10.1002/term.1759

PubMed Abstract | CrossRef Full Text | Google Scholar

Azerêdo, M. S., Nunes, M. A. B. S., Figueiredo, L. R. F., Oliveira, J. E., Tonoli, G. D., de Barros, S., et al. (2022). Environmentally friendly adhesives derived from glycerol-based polymers. J. Adhes. Sci. Technol. 36, 98–108. doi:10.1080/01694243.2021.1915619

CrossRef Full Text | Google Scholar

Behtaj, S., Karamali, F., Masaeli, E., Anissimov, G. Y., and Rybachuk, M. (2021). Electrospun PGS/PCL, PLLA/PCL, PLGA/PCL and pure PCL scaffolds for retinal progenitor cell cultivation. Biochem. Eng. J. 166, 107846. doi:10.1016/j.bej.2020.107846

CrossRef Full Text | Google Scholar

Behtaj, S., Karamali, F., Najafian, S., Masaeli, E., Esfahani, M. H. N., and Rybachuk, M. (2021). The role of PGS/PCL scaffolds in promoting differentiation of human embryonic stem cells into retinal ganglion cells. Acta Biomater. 126, 238–248. doi:10.1016/j.actbio.2021.03.036

PubMed Abstract | CrossRef Full Text | Google Scholar

Behtouei, E., Zandi, M., Askari, F., Daemi, H., Zamanlui, S., Arabsorkhi-Mishabi, A., et al. (2022). Bead-free and tough electrospun PCL/gelatin/PGS ternary nanofibrous scaffolds for tissue engineering application. J. Appl. Polym. Sci. 139, 51471. doi:10.1002/app.51471

CrossRef Full Text | Google Scholar

Bellani, C. F., Yue, K., Flaig, F., Hebraud, A., Ray, P., Annabi, N., et al. (2021). Suturable elastomeric tubular grafts with patterned porosity for rapid vascularization of 3D constructs. Biofabrication 13, 035020. doi:10.1088/1758-5090/abdf1d

PubMed Abstract | CrossRef Full Text | Google Scholar

Cai, W., and Liu, L. (2007). Shape-memory effect of poly (glycerol–sebacate) elastomer. Mat. Lett. 62, 2171–2173. doi:10.1016/j.matlet.2007.11.042

CrossRef Full Text | Google Scholar

Chang, C., and Yeh, Y. (2021). Poly(glycerol sebacate) co-poly(ethylene glycol)/gelatin hybrid hydrogels as biocompatible biomaterials for cell proliferation and Spreading. Macromol. Biosci. 21, 2100248. doi:10.1002/mabi.202100248

PubMed Abstract | CrossRef Full Text | Google Scholar

Chang, P.-Y., Wang, J., Li, S.-Y., and Suen, S.-Y. (2021). Biodegradable polymeric membranes for organic solvent/water pervaporation applications. Membr. (Basel). 11, 970. doi:10.3390/membranes11120970

PubMed Abstract | CrossRef Full Text | Google Scholar

Chen, J.-Y., Hwang, J., Ao-Ieong, W. S., Lin, Y. C., Hsieh, Y. K., Cheng, Y. L., et al. (2018). Study of physical and degradation properties of 3D-printed biodegradable, photocurable copolymers, PGSA-co-PEGDA and PGSA-co-PCLDA. Polym. (Basel). 10, 1263. doi:10.3390/polym10111263

PubMed Abstract | CrossRef Full Text | Google Scholar

Chen, Q.-Z., Bismarck, A., Hansen, U., Junaid, S., Tran, M. Q., Harding, S. E., et al. (2007). Characterisation of a soft elastomer poly(glycerol sebacate) designed to match the mechanical properties of myocardial tissue. Biomaterials 29, 47–57. doi:10.1016/j.biomaterials.2007.09.010

PubMed Abstract | CrossRef Full Text | Google Scholar

Chen, Q., Jin, L., Cook, W. D., Mohn, D., Lagerqvist, E. L., Elliott, D. A., et al. (2010). Elastomeric nanocomposites as cell delivery vehicles and cardiac support devices. Soft Matter 6, 4715. doi:10.1039/c0sm00213e

CrossRef Full Text | Google Scholar

Chen, Q., Liang, S., and Thouas, G. A. (2011). Synthesis and characterisation of poly(glycerol sebacate)-co-lactic acid as surgical sealants. Soft Matter 7, 6484. doi:10.1039/c1sm05350g

CrossRef Full Text | Google Scholar

Chen, S., Bi, X., Sun, L., Gao, J., Huang, P., Fan, X., et al. (2016). Poly(sebacoyl diglyceride) cross-linked by dynamic hydrogen bonds: A self-healing and functionalizable thermoplastic Bioelastomer. ACS Appl. Mat. Interfaces 8, 20591–20599. doi:10.1021/acsami.6b05873

PubMed Abstract | CrossRef Full Text | Google Scholar

Chen, S., Huang, T., Zuo, H., Qian, S., Guo, Y., Sun, L., et al. (2018). Wearable electronics: A single integrated 3D-printing process Customizes elastic and sustainable Triboelectric Nanogenerators for Wearable electronics (Adv. Funct. Mater. 46/2018). Adv. Funct. Mat. 28, 1870331. doi:10.1002/adfm.201870331

CrossRef Full Text | Google Scholar

Chen, W., Xiao, W., Liu, X., Yuan, P., Zhang, S., Wang, Y., et al. (2022). Pharmacological manipulation of macrophage autophagy effectively rejuvenates the regenerative potential of biodegrading vascular graft in aging body. Bioact. Mat. 11, 283–299. doi:10.1016/j.bioactmat.2021.09.027

PubMed Abstract | CrossRef Full Text | Google Scholar

Choi, I., and Yoon, K. (2010). Process of preparing A biodegradable polymer using an enzyme catalyst and A biodegradable polymer prepared through the process. US7642075B2. United States.

Google Scholar

Choi, S. M., Lee, Y., Son, J. Y., Bae, J. W., Park, K. M., and Park, K. D. (2017). Synthesis and characterization of in situ gellable poly(glycerol sebacate)-co-poly(ethylene glycol) polymers. Macromol. Res. 25, 85–91. doi:10.1007/s13233-017-5007-y

CrossRef Full Text | Google Scholar

Coativy, G., Misra, M., and Mohanty, A. K. (2016). Microwave synthesis and Melt blending of glycerol based toughening agent with poly(lactic acid). ACS Sustain. Chem. Eng. 4, 2142–2149. doi:10.1021/acssuschemeng.5b01596

CrossRef Full Text | Google Scholar

Coativy, G., Misra, M., and Mohanty, A. K. (2017). Synthesis of shape memory poly(glycerol sebacate)-Stearate polymer. Macromol. Mat. Eng. 302, 1600294–1600296. doi:10.1002/mame.201600294

CrossRef Full Text | Google Scholar

Conejero-García, Á., Gimeno, H. R., Saez, Y. M., Vilarino-Feltrer, G., Ortuno-Lizaran, I., and Valles-Lluch, A. (2017). Correlating synthesis parameters with physicochemical properties of poly(glycerol sebacate). Eur. Polym. J. 87, 406–419. doi:10.1016/j.eurpolymj.2017.01.001

CrossRef Full Text | Google Scholar

Davoodi, B., Goodarzi, V., Hosseini, H., Tirgar, M., Shojaei, S., Asefnejad, A., et al. (2022). Design and manufacturing a tubular structures based on poly(ɛ-caprolactone)/poly(glycerol-sebacic acid) biodegradable nanocomposite blends: Suggested for applications in the nervous, vascular and renal tissue engineering. J. Polym. Res. 29, 54. doi:10.1007/s10965-021-02881-8

CrossRef Full Text | Google Scholar

Deniz, P., Guler, S., Çelik, E., Hosseinian, P., and Aydin, H. M. (2020). Use of cyclic strain bioreactor for the upregulation of key tenocyte gene expression on Poly(glycerol-sebacate) (PGS) sheets. Mater. Sci. Eng. C 106, 110293. doi:10.1016/j.msec.2019.110293

PubMed Abstract | CrossRef Full Text | Google Scholar

Desai, P., Venkataramanan, A., Schneider, R., Jaiswal, M. K., Carrow, J. K., Purwada, A., et al. (2018). Self-assembled, ellipsoidal polymeric nanoparticles for intracellular delivery of therapeutics. J. Biomed. Mat. Res. A 106, 2048–2058. doi:10.1002/jbm.a.36400

PubMed Abstract | CrossRef Full Text | Google Scholar

Ding, X., Chen, Y., Chao, C. A., Wu, Y., and Wang, Y. (2020). Control the mechanical properties and degradation of poly(glycerol sebacate) by substitution of the hydroxyl groups with palmitates. Macromol. Biosci. 20, 2000101. doi:10.1002/mabi.202000101

PubMed Abstract | CrossRef Full Text | Google Scholar

Ding, X., Wu, Y. L., Gao, J., Wells, A., Lee, K. W., and Wang, Y. (2017). Tyramine functionalization of poly(glycerol sebacate) increases the elasticity of the polymer. J. Mat. Chem. B 5, 6097–6109. doi:10.1039/c7tb01078h

PubMed Abstract | CrossRef Full Text | Google Scholar

Fakhari, Z., Nouri Khorasani, S., Alihosseini, F., Nasr Esfahani, M. H., Karamali, F., and Khalili, S. (2021). Core–shell nanofibers of poly (glycerol sebacate) and poly (1, 8 octanediol citrate) for retinal regeneration. Polym. Bull. 79, 7161–7176. doi:10.1007/s00289-021-03850-3

CrossRef Full Text | Google Scholar

Fakhrali, A., Nasari, M., Poursharifi, N., Semnani, D., Salehi, H., Ghane, M., et al. (2021). Biocompatible graphene-embedded PCL/PGS-based nanofibrous scaffolds: A potential application for cardiac tissue regeneration. J. Appl. Polym. Sci. 138, 51177. doi:10.1002/app.51177

CrossRef Full Text | Google Scholar

Fakhrali, A., Semnani, D., Salehi, H., and Ghane, M. (2022). Electro-conductive nanofibrous structure based on PGS/PCL coated with PPy by in situ chemical polymerization applicable as cardiac patch: Fabrication and optimization. J. Appl. Polym. Sci. 139, 52136. doi:10.1002/app.52136

CrossRef Full Text | Google Scholar

Fakhrali, A., Semnani, D., Salehi, H., and Ghane, M. (2020). Electrospun PGS/PCL nanofibers: From straight to sponge and spring-like morphology. Polym. Adv. Technol. 31, 3134–3149. doi:10.1002/pat.5038

CrossRef Full Text | Google Scholar

Farr, N., Pashneh-Tala, S., Stehling, N., Claeyssens, F., Green, N., and Rodenburg, C. (2020). Characterizing cross-linking within polymeric biomaterials in the SEM by secondary Electron Hyperspectral imaging. Macromol. Rapid Commun. 41, 2070006. doi:10.1002/marc.202070006

PubMed Abstract | CrossRef Full Text | Google Scholar

Flaig, F., Bellani, C. F., Uyumaz, Ö., Schlatter, G., and Hébraud, A. (2021). Elaboration and mechanical properties of elastomeric fibrous scaffolds based on crosslinked poly(glycerol sebacate) and cyclodextrin for soft tissue engineering. Mat. Adv. 2, 1284–1293. doi:10.1039/d0ma00673d

CrossRef Full Text | Google Scholar

Flaig, F., Ragot, H., Simon, A., Revet, G., Kitsara, M., Kitasato, L., et al. (2020). Design of functional electrospun scaffolds based on poly(glycerol sebacate) elastomer and poly(lactic acid) for cardiac tissue engineering. ACS Biomater. Sci. Eng. 6, 2388–2400. doi:10.1021/acsbiomaterials.0c00243

PubMed Abstract | CrossRef Full Text | Google Scholar

Frydrych, M., and Chen, B. (2017). Fabrication, structure and properties of three-dimensional biodegradable poly(glycerol sebacate urethane) scaffolds. Polymer 122, 159–168. doi:10.1016/j.polymer.2017.06.064

CrossRef Full Text | Google Scholar

Frydrych, M., Román, S., Green, N. H., MacNeil, S., and Chen, B. (2015). Thermoresponsive, stretchable, biodegradable and biocompatible poly(glycerol sebacate)-based polyurethane hydrogels. Polym. Chem. 6, 7974–7987. doi:10.1039/c5py01136a

CrossRef Full Text | Google Scholar

Frydrych, M., Román, S., MacNeil, S., and Chen, B. (2015). Biomimetic poly(glycerol sebacate)/poly(l-lactic acid) blend scaffolds for adipose tissue engineering. Acta Biomater. 18, 40–49. doi:10.1016/j.actbio.2015.03.004

PubMed Abstract | CrossRef Full Text | Google Scholar

Fu, J., Ding, X., Stowell, C. E. T., Wu, Y.-L., and Wang, Y. (2020). Slow degrading poly(glycerol sebacate) derivatives improve vascular graft remodeling in a rat carotid artery interposition model. Biomaterials 257, 120251. doi:10.1016/j.biomaterials.2020.120251

PubMed Abstract | CrossRef Full Text | Google Scholar

Fu, J., Wang, M., De Vlaminck, I., and Wang, Y. (2020). Thick PCL fibers improving host remodeling of PGS-PCL composite grafts implanted in rat common carotid arteries. Small 16, 2004133. doi:10.1002/smll.202004133

PubMed Abstract | CrossRef Full Text | Google Scholar

Fukunishi, T., Lui, C., Ong, C. S., Dunn, T., Xu, S., Smoot, C., et al. (2022). Extruded poly (glycerol sebacate) and polyglycolic acid vascular graft forms a neoartery. J. Tissue Eng. Regen. Med. 16, 346–354. doi:10.1002/term.3282

PubMed Abstract | CrossRef Full Text | Google Scholar

Gadomska-Gajadhur, A., Wrzecionek, M., Matyszczak, G., Pietowski, P., Wieclaw, M., and Ruskowski, P. (2018). Optimization of poly(glycerol sebacate) synthesis for biomedical purposes with the design of experiments. Org. Process Res. Dev. 22, 1793–1800. doi:10.1021/acs.oprd.8b00306

CrossRef Full Text | Google Scholar

Gaharwar, A. K., Patel, A., Dolatshahi-Pirouz, A., Zhang, H., Rangarajan, K., Iviglia, G., et al. (2015). Elastomeric nanocomposite scaffolds made from poly(glycerol sebacate) chemically crosslinked with carbon nanotubes. Biomater. Sci. 3, 46–58. doi:10.1039/c4bm00222a

PubMed Abstract | CrossRef Full Text | Google Scholar

Gao, J., Crapo, P. M., and Wang, Y. (2006). Macroporous elastomeric scaffolds with extensive micropores for soft tissue engineering. Tissue Eng. 12, 917–925. doi:10.1089/ten.2006.12.917

PubMed Abstract | CrossRef Full Text | Google Scholar

Gao, J., Ensley, A. E., Nerem, R. M., and Wang, Y. (2007). Poly(glycerol sebacate) supports the proliferation and phenotypic protein expression of primary baboon vascular cells. J. Biomed. Mat. Res. A 83A, 1070–1075. doi:10.1002/jbm.a.31434

PubMed Abstract | CrossRef Full Text | Google Scholar

Ghafarzadeh, M., Kharaziha, M., and Atapour, M. (2021). Bilayer micro-arc oxidation-poly (glycerol sebacate) coating on AZ91 for improved corrosion resistance and biological activity. Prog. Org. Coat. 161, 106495. doi:10.1016/j.porgcoat.2021.106495

CrossRef Full Text | Google Scholar

Godinho, B., Gama, N., Barros-Timmons, A., and Ferreira, A. (2018). “Enzymatic synthesis of poly(glycerol sebacate) pre-polymer with crude glycerol, by-product from biodiesel prodution,” in AIP Conference Proceedings, Ischia, Italy, July 2018 (AIP Publishing LLC), 020031.

CrossRef Full Text | Google Scholar

Golbaten-Mofrad, H., Seyfi Sahzabi, A., Seyfikar, S., Salehi, M. H., Goodarzi, V., Wurm, F. R., et al. (2021). Facile template preparation of novel electroactive scaffold composed of polypyrrole-coated poly(glycerol-sebacate-urethane) for tissue engineering applications. Eur. Polym. J. 159, 110749. doi:10.1016/j.eurpolymj.2021.110749

CrossRef Full Text | Google Scholar

Gorgani, S., Zargar Kharazi, A., Haghjooy Javanmard, S., and Rafiinia, M. (2020). Improvement of endothelial cell performance in an optimized electrospun pre-polyglycerol sebacate-poly lactic acid scaffold for Reconstruction of Intima in Coronary arteries. J. Polym. Environ. 28, 2352–2363. doi:10.1007/s10924-020-01749-0

CrossRef Full Text | Google Scholar

Gultekinoglu, M., Öztürk, Ş., Chen, B., Edirisinghe, M., and Ulubayram, K. (2019). Preparation of poly(glycerol sebacate) fibers for tissue engineering applications. Eur. Polym. J. 121, 109297. doi:10.1016/j.eurpolymj.2019.109297

CrossRef Full Text | Google Scholar

Guo, X.-L., Lu, X.-L., Dong, D.-L., and Sun, Z.-J. (2014). Characterization and optimization of glycerol/sebacate ratio in poly(glycerol-sebacate) elastomer for cell culture application. J. Biomed. Mat. Res. A 102, 3903–3907. doi:10.1002/jbm.a.35066

PubMed Abstract | CrossRef Full Text | Google Scholar

Halil Murat, A. (2017). Poly(Glycerol-Sebacate) elastomer: A Mini review. Orthoplastic Surg. Orthop. Care Int. J. 1. doi:10.31031/ooij.2017.01.000507

CrossRef Full Text | Google Scholar

Hanif, A., Ghosh, G., Meeseepong, M., Haq Chouhdry, H., Bag, A., Chinnamani, M., et al. (2021). A composite microfiber for biodegradable stretchable electronics. Micromachines 12, 1036. doi:10.3390/mi12091036

PubMed Abstract | CrossRef Full Text | Google Scholar

Heydari, P., Zargar Kharazi, A., Asgary, S., and Parham, S. (2022). Comparing the wound healing effect of a controlled release wound dressing containing curcumin/ciprofloxacin and simvastatin/ciprofloxacin in a rat model: A preclinical study. J. Biomed. Mat. Res. A 110, 341–352. doi:10.1002/jbm.a.37292

PubMed Abstract | CrossRef Full Text | Google Scholar

Hou, L., Zhang, X., Mikael, P. E., Lin, L., Dong, W., Zheng, Y., et al. (2017). Biodegradable and Bioactive PCL-PGS core-shell fibers for tissue engineering. ACS Omega 2, 6321–6328. doi:10.1021/acsomega.7b00460

PubMed Abstract | CrossRef Full Text | Google Scholar

Hsu, C.-N., Lee, P.-Y., Tuan-Mu, H.-Y., Li, C.-Y., and Hu, J.-J. (2018). Fabrication of a mechanically anisotropic poly(glycerol sebacate) membrane for tissue engineering. J. Biomed. Mat. Res. 106, 760–770. doi:10.1002/jbm.b.33876

PubMed Abstract | CrossRef Full Text | Google Scholar

Hu, J., Kai, D., Ye, H., Tian, L., Ding, X., Ramakrishna, S., et al. (2017). Electrospinning of poly(glycerol sebacate)-based nanofibers for nerve tissue engineering. Mater. Sci. Eng. C 70, 1089–1094. doi:10.1016/j.msec.2016.03.035

PubMed Abstract | CrossRef Full Text | Google Scholar

Hu, T., Wu, Y., Zhao, X., Wang, L., Bi, L., Ma, P. X., et al. (2019). Micropatterned, electroactive, and biodegradable poly(glycerol sebacate)-aniline trimer elastomer for cardiac tissue engineering. Chem. Eng. J. 366, 208–222. doi:10.1016/j.cej.2019.02.072

CrossRef Full Text | Google Scholar

Ifkovits, J. L., Padera, R. F., and Burdick, J. A. (2008). Biodegradable and radically polymerized elastomers with enhanced processing capabilities. Biomed. Mat. 3, 034104. doi:10.1088/1748-6041/3/3/034104

PubMed Abstract | CrossRef Full Text | Google Scholar

Jaafar, I. H., Ammar, M. M., Jedlicka, S. S., Pearson, R. A., and Coulter, J. P. (2010). Spectroscopic evaluation, thermal, and thermomechanical characterization of poly(glycerol-sebacate) with variations in curing temperatures and durations. J. Mat. Sci. 45, 2525–2529. doi:10.1007/s10853-010-4259-0

CrossRef Full Text | Google Scholar

Jafari, Fatemeh, Khorasani, S. N., Alihosseini, F., Semnani, D., Khalili, S., and Neisiany, R. E. (2020). Development of an electrospun scaffold for retinal tissue engineering. Polym. Sci. Ser. B 62, 290–298. doi:10.1134/s1560090420030069

CrossRef Full Text | Google Scholar

Jeffries, E. M., Allen, R. a., Gao, J., Pesce, M., and Wang, Y. (2015). Highly elastic and suturable electrospun poly(glycerol sebacate) fibrous scaffolds. Acta Biomater. 18, 30–39. doi:10.1016/j.actbio.2015.02.005

PubMed Abstract | CrossRef Full Text | Google Scholar

Jeong, C. G., and Hollister, S. J. (2010). A comparison of the influence of material on in vitro cartilage tissue engineering with PCL, PGS, and POC 3D scaffold architecture seeded with chondrocytes. Biomaterials 31, 4304–4312. doi:10.1016/j.biomaterials.2010.01.145

PubMed Abstract | CrossRef Full Text | Google Scholar

Jia, Y., Wang, W., Zhou, X., Nie, W., and Chen, L. (2016). Synthesis and characterization of poly(glycerol sebacate)-based elastomeric copolyesters for tissue engineering applications. Polym. Chem. 7, 2553–2564. doi:10.1039/c5py01993a

CrossRef Full Text | Google Scholar

Jiang, L., Jiang, Y., Stiadle, J., Wang, X., Wang, L., Li, Q., et al. (2019). Electrospun nanofibrous thermoplastic polyurethane/poly(glycerol sebacate) hybrid scaffolds for vocal fold tissue engineering applications. Mater. Sci. Eng. C 94, 740–749. doi:10.1016/j.msec.2018.10.027

PubMed Abstract | CrossRef Full Text | Google Scholar

Jiang, W., Zhang, C., Tran, L., Wang, S. G., Hakim, A. D., and Liu, H. (2020). Engineering Nano-to-Micron-patterned polymer coatings on bioresorbable Magnesium for controlling human endothelial cell adhesion and morphology. ACS Biomater. Sci. Eng. 6, 3878–3898. doi:10.1021/acsbiomaterials.0c00642

PubMed Abstract | CrossRef Full Text | Google Scholar

Kafouris, D., Kossivas, F., Constantinides, C., Nguyen, N. Q., Wesdemiotis, C., and Patrickios, C. S. (2013). Biosourced amphiphilic degradable elastomers of poly(glycerol sebacate): Synthesis and network and oligomer characterization. Macromolecules 46, 622–630. doi:10.1021/ma3016882

CrossRef Full Text | Google Scholar

Kaya, M., Ahi, Z. B., Ergene, E., Yilgor Huri, P., and Tuzlakoglu, K. (2020). Design of a new dual mesh with an absorbable nanofiber layer as a potential implant for abdominal hernia treatment. J. Tissue Eng. Regen. Med. 14, 347–354. doi:10.1002/term.3000

PubMed Abstract | CrossRef Full Text | Google Scholar

Kazemzadeh Farizhandi, A. A., Khalajabadi, S. Z., Krishnadoss, V., and Noshadi, I. (2020). Synthesized biocompatible and conductive ink for 3D printing of flexible electronics. J. Mech. Behav. Biomed. Mat. 110, 103960. doi:10.1016/j.jmbbm.2020.103960

PubMed Abstract | CrossRef Full Text | Google Scholar

Keirouz, A., Zakharova, M., Kwon, J., Robert, C., Koutsos, V., Callanan, A., et al. (2020). High-throughput production of silk fibroin-based electrospun fibers as biomaterial for skin tissue engineering applications. Mater. Sci. Eng. C 112, 110939. doi:10.1016/j.msec.2020.110939

PubMed Abstract | CrossRef Full Text | Google Scholar

Kemppainen, J. M., and Hollister, S. J. (2010). Tailoring the mechanical properties of 3D-designed poly(glycerol sebacate) scaffolds for cartilage applications. J. Biomed. Mat. Res. A 94A, 9–18. doi:10.1002/jbm.a.32653

PubMed Abstract | CrossRef Full Text | Google Scholar

Khosravi, R., Best, C. A., Allen, R. A., Stowell, C. E. T., Onwuka, E., Zhuang, J. J., et al. (2016). Long-term functional Efficacy of a novel electrospun poly(glycerol sebacate)-based arterial graft in mice. Ann. Biomed. Eng. 44, 2402–2416. doi:10.1007/s10439-015-1545-7

PubMed Abstract | CrossRef Full Text | Google Scholar

Kim, M. J., Hwang, M. Y., Kim, J., and Chung, D. J. (2014). Biodegradable and elastomeric poly(glycerol sebacate) as a coating material for nitinol bare stent. Biomed. Res. Int. 2014, 1–7. doi:10.1155/2014/956952

PubMed Abstract | CrossRef Full Text | Google Scholar

Kobayashi, S. (2010). Lipase-catalyzed polyester synthesis-a green polymer chemistry. Proc. Jpn. Acad. Ser. B. Phys. Biol. Sci. 86, 338–365. doi:10.2183/pjab.86.338

PubMed Abstract | CrossRef Full Text | Google Scholar

Kossivas, F., Angeli, S., Kafouris, D., Patrickios, C. S., Tzagarakis, V., and Constantinides, C. (2012). MRI-based morphological modeling, synthesis and characterization of cardiac tissue-mimicking materials. Biomed. Mat. 7, 035006. doi:10.1088/1748-6041/7/3/035006

PubMed Abstract | CrossRef Full Text | Google Scholar

Krook, N. M., Jaafar, I. H., Sarkhosh, T., LeBlon, C., Coulter, J. P., and Jedlicka, S. S. (2020). In vitro examination of poly(glycerol sebacate) degradation kinetics: Effects of porosity and cure temperature. Int. J. Polym. Mater. Polym. Biomaterials 69, 535–543. doi:10.1080/00914037.2019.1596907

CrossRef Full Text | Google Scholar

Lang, K., Bhattacharya, S., Ning, Z., Sanchez-Leija, R. J., Bramson, M. T. K., Centore, R., et al. (2020). Enzymatic polymerization of poly(glycerol-1, 8-octanediol-sebacate): Versatile poly(glycerol sebacate) Analogues that form Monocomponent biodegradable fiber scaffolds. Biomacromolecules 21, 3197–3206. doi:10.1021/acs.biomac.0c00641

PubMed Abstract | CrossRef Full Text | Google Scholar

Lau, C. C., Al Qaysi, M., Owji, N., Bayazit, M., Xie, J., Knowles, J., et al. (2020). Advanced biocomposites of poly(glycerol sebacate) and β-tricalcium phosphate by in situ microwave synthesis for bioapplication. Mat. Today Adv. 5, 100023. doi:10.1016/j.mtadv.2019.100023

CrossRef Full Text | Google Scholar

Lau, C. C., Bayazit, M. K., Knowles, J. C., and Tang, J. (2017). Tailoring degree of esterification and branching of poly(glycerol sebacate) by energy efficient microwave irradiation. Polym. Chem. 8, 3937–3947. doi:10.1039/c7py00862g

CrossRef Full Text | Google Scholar

Lee, S. H., Lee, K.-W., Gade, P. S., Robertson, A. M., and Wang, Y. (2018). Microwave-assisted facile fabrication of porous poly (glycerol sebacate) scaffolds. J. Biomaterials Sci. Polym. Ed. 29, 907–916. doi:10.1080/09205063.2017.1335076

PubMed Abstract | CrossRef Full Text | Google Scholar

Li, X., Hong, A. T.-L., Naskar, N., and Chung, H.-J. (2015). Criteria for quick and consistent synthesis of poly(glycerol sebacate) for tailored mechanical properties. Biomacromolecules 16, 1525–1533. doi:10.1021/acs.biomac.5b00018

PubMed Abstract | CrossRef Full Text | Google Scholar

Li, Y., Cook, W. D., Moorhoff, C., Huang, W.-C., and Chen, Q.-Z. (2013). Synthesis, characterization and properties of biocompatible poly(glycerol sebacate) pre-polymer and gel. Polym. Int. 62, 534–547. doi:10.1002/pi.4419

CrossRef Full Text | Google Scholar

Li, Y., Huang, W., Cook, W. D., and Chen, Q. (2013). A comparative study on poly(xylitol sebacate) and poly(glycerol sebacate): Mechanical properties, biodegradation and cytocompatibility. Biomed. Mat. 8, 035006. doi:10.1088/1748-6041/8/3/035006

PubMed Abstract | CrossRef Full Text | Google Scholar

Liang, B., Shi, Q., Xu, J., Chai, Y.-M., and Xu, J.-G. (2020). Poly (glycerol sebacate)-based bio-artificial Multiporous matrix for bone regeneration. Front. Chem. 8, 603577. doi:10.3389/fchem.2020.603577

PubMed Abstract | CrossRef Full Text | Google Scholar

Liang, S., Cook, W. D., and Chen, Q. (2011). Physical characterization of poly(glycerol sebacate)/Bioglass ® composites. Polym. Int. 61, 17–22. doi:10.1002/pi.3165

CrossRef Full Text | Google Scholar

Lin, D., Yang, K., Tang, W., Liu, Y., Yuan, Y., and Liu, C. (2015). A poly(glycerol sebacate)-coated mesoporous bioactive glass scaffold with adjustable mechanical strength, degradation rate, controlled-release and cell behavior for bone tissue engineering. Colloids Surfaces B Biointerfaces 131, 1–11. doi:10.1016/j.colsurfb.2015.04.031

PubMed Abstract | CrossRef Full Text | Google Scholar

Liu, Q., Tian, M., Ding, T., Shi, R., Feng, Y., Zhang, L., et al. (2007). Preparation and characterization of a thermoplastic poly(glycerol sebacate) elastomer by two-step method. J. Appl. Polym. Sci. 103, 1412–1419. doi:10.1002/app.24394

CrossRef Full Text | Google Scholar

Liu, Q., Tian, M., Shi, R., Zhang, L., Chen, D., and Tian, W. (2007). Structure and properties of thermoplastic poly(glycerol sebacate) elastomers originating from prepolymers with different molecular weights. J. Appl. Polym. Sci. 104, 1131–1137. doi:10.1002/app.25606

CrossRef Full Text | Google Scholar

Liu, Q., Wu, J., Tan, T., Zhang, L., Chen, D., and Tian, W. (2009). Preparation, properties and cytotoxicity evaluation of a biodegradable polyester elastomer composite. Polym. Degrad. Stab. 94, 1427–1435. doi:10.1016/j.polymdegradstab.2009.05.023

CrossRef Full Text | Google Scholar

Liu, X., Chen, W., Shao, B., Zhang, X., Wang, Y., Zhang, S., et al. (2021). Mussel patterned with 4D biodegrading elastomer durably recruits regenerative macrophages to promote regeneration of craniofacial bone. Biomaterials 276, 120998. doi:10.1016/j.biomaterials.2021.120998

PubMed Abstract | CrossRef Full Text | Google Scholar

Loh, X. J., Abdul Karim, A., and Owh, C. (2015). Poly(glycerol sebacate) biomaterial: Synthesis and biomedical applications. J. Mat. Chem. B 3, 7641–7652. doi:10.1039/c5tb01048a

PubMed Abstract | CrossRef Full Text | Google Scholar

Luginina, M., Schuhladen, K., Orru, R., Cao, G., Boccaccini, A. R., and Liverani, L. (2020). Electrospun PCL/PGS composite fibers incorporating bioactive glass Particles for soft tissue engineering applications. Nanomaterials 10, 978. doi:10.3390/nano10050978

PubMed Abstract | CrossRef Full Text | Google Scholar

Ma, Y., Zhang, W., Wang, Z., Wang, Z., Xie, Q., Niu, H., et al. (2016). PEGylated poly(glycerol sebacate)-modified calcium phosphate scaffolds with desirable mechanical behavior and enhanced osteogenic capacity. Acta Biomater. 44, 110–124. doi:10.1016/j.actbio.2016.08.023

PubMed Abstract | CrossRef Full Text | Google Scholar

Mahdavi, A., Ferreira, L., Sundback, C., Nichol, J. W., Chan, E. P., Carter, D. J. D., et al. (2008). A biodegradable and biocompatible gecko-inspired tissue adhesive. Proc. Natl. Acad. Sci. U. S. A. 105, 2307–2312. doi:10.1073/pnas.0712117105

PubMed Abstract | CrossRef Full Text | Google Scholar

Maliger, R., Halley, P. J., and Cooper-White, J. J. (2013). Poly(glycerol-sebacate) bioelastomers-kinetics of step-growth reactions using Fourier Transform (FT)-Raman spectroscopy. J. Appl. Polym. Sci. 127, 3980–3986. doi:10.1002/app.37719

CrossRef Full Text | Google Scholar

Martín-Cabezuelo, R., Rodríguez-Hernández, J. C., Vilariño-Feltrer, G., and Vallés-Lluch, A. (2021). Role of curing temperature of poly(glycerol sebacate) Substrates on protein-cell interaction and early cell adhesion. Polym. (Basel). 13, 382. doi:10.3390/polym13030382

PubMed Abstract | CrossRef Full Text | Google Scholar

Martín-Cabezuelo, R., Vilariño-Feltrer, G., and Vallés-Lluch, A. (2021). Influence of pre-polymerisation atmosphere on the properties of pre- and poly(glycerol sebacate). Mater. Sci. Eng. C 119, 111429. doi:10.1016/j.msec.2020.111429

PubMed Abstract | CrossRef Full Text | Google Scholar

Martín-Pat, G. E., Rodriguez-Fuentes, N., Cervantes-Uc, J. M., Rosales-Ibanez, R., Carrillo-Escalante, H. J., Ku-Gonzalez, A. F., et al. (2020). Effect of different exposure times on physicochemical, mechanical and biological properties of PGS scaffolds treated with plasma of iodine-doped polypyrrole. J. Biomater. Appl. 35, 485–499. doi:10.1177/0885328220941466

PubMed Abstract | CrossRef Full Text | Google Scholar

Masoumi, N., Jean, A., Zugates, J. T., Johnson, K. L., and Engelmayr, G. C. (2013). Laser microfabricated poly(glycerol sebacate) scaffolds for heart valve tissue engineering. J. Biomed. Mat. Res. A 101A, 104–114. doi:10.1002/jbm.a.34305

PubMed Abstract | CrossRef Full Text | Google Scholar

Matyszczak, G., Wrzecionek, M., Gadomska-Gajadhur, A., and Ruśkowski, P. (2020). Kinetics of polycondensation of sebacic acid with glycerol. Org. Process Res. Dev. 24, 1104–1111. doi:10.1021/acs.oprd.0c00110

CrossRef Full Text | Google Scholar

McKee, C. T., Last, J. A., Russell, P., and Murphy, C. J. (2011). Indentation versus tensile measurements of Young’s modulus for soft biological tissues. Tissue Eng. Part B Rev. 17, 155–164. doi:10.1089/ten.teb.2010.0520

PubMed Abstract | CrossRef Full Text | Google Scholar

Mehta, M., Zhao, C., Liu, A., Innocent, C., and Kohane, D. S. (2022). Prolonged Retrobulbar local Anesthesia of the cornea does not cause Keratopathy in mice. Transl. Vis. Sci. Technol. 11, 33. doi:10.1167/tvst.11.1.33

PubMed Abstract | CrossRef Full Text | Google Scholar

Mitsak, A. G., Dunn, A. M., and Hollister, S. J. (2012). Mechanical characterization and non-linear elastic modeling of poly(glycerol sebacate) for soft tissue engineering. J. Mech. Behav. Biomed. Mat. 11, 3–15. doi:10.1016/j.jmbbm.2011.11.003

PubMed Abstract | CrossRef Full Text | Google Scholar

Mokhtari, N., and Zargar Kharazi, A. (2021). Blood compatibility and cell response improvement of poly glycerol sebacate/poly lactic acid scaffold for vascular graft applications. J. Biomed. Mat. Res. A 109, 2673–2684. doi:10.1002/jbm.a.37259

PubMed Abstract | CrossRef Full Text | Google Scholar

Monem, M., Ahmadi, Z., Fakhri, V., and Goodarzi, V. (2022). Preparing and characterization of poly(glycerol-sebacic acid-urethane) (PGSU) nanocomposites: Clearing role of unmodified and modified clay nanoparticles. J. Polym. Res. 29, 25. doi:10.1007/s10965-021-02866-7

CrossRef Full Text | Google Scholar

Moorhoff, C., Li, Y., Cook, W. D., Braybrook, C., and Chen, Q.-Z. (2015). Characterization of the prepolymer and gel of biocompatible poly(xylitol sebacate) in comparison with poly(glycerol sebacate) using a combination of mass spectrometry and nuclear magnetic resonance. Polym. Int. 64, 668–688. doi:10.1002/pi.4831

CrossRef Full Text | Google Scholar

Nadim, A., Khorasani, S. N., Kharaziha, M., and Davoodi, S. M. (2017). Design and characterization of dexamethasone-loaded poly (glycerol sebacate)-poly caprolactone/gelatin scaffold by coaxial electro spinning for soft tissue engineering. Mater. Sci. Eng. C 78, 47–58. doi:10.1016/j.msec.2017.04.047

PubMed Abstract | CrossRef Full Text | Google Scholar

Nagata, M., Kiyotsukuri, T., Ibuki, H., Tsutsumi, N., and Sakai, W. (1996). Synthesis and enzymatic degradation of regular network aliphatic polyesters. React. Funct. Polym. 30, 165–171. doi:10.1016/1381-5148(95)00107-7

CrossRef Full Text | Google Scholar

Nagata, M., Machida, T., Sakai, W., and Tsutsumi, N. (1999). Synthesis, characterization, and enzymatic degradation of network aliphatic copolyesters. J. Polym. Sci. A. Polym. Chem. 37, 2005–2011. doi:10.1002/(sici)1099-0518(19990701)37:13<2005:aid-pola14>3.0.co;2-h

CrossRef Full Text | Google Scholar

Nijst, C. L. E., Bruggeman, J. P., Karp, J. M., Ferreira, L., Zumbuehl, A., Bettinger, C. J., et al. (2007). Synthesis and characterization of photocurable elastomers from poly(glycerol-co-sebacate). Biomacromolecules 8, 3067–3073. doi:10.1021/bm070423u

PubMed Abstract | CrossRef Full Text | Google Scholar

Ning, Z., Lang, K., Xia, K., Linhardt, R. J., and Gross, R. A. (2022). Lipase-catalyzed synthesis and characterization of poly(glycerol sebacate). Biomacromolecules 23, 398–408. doi:10.1021/acs.biomac.1c01351

PubMed Abstract | CrossRef Full Text | Google Scholar

Oklu, R., Rezaei Nejad, H., Chen, A. Z., Ju, J., Tamayol, A., Liu, X., et al. (2018). Fracture-resistant and bioresorbable drug-Eluting poly(glycerol sebacate) coils. Adv. Ther. (Weinh). 2 (3), 1800109. doi:10.1002/adtp.201800109

CrossRef Full Text | Google Scholar

Pan, Q., Guo, Y., and Kong, F. (2018). Poly(glycerol sebacate) combined with chondroitinase ABC promotes spinal cord repair in rats. J. Biomed. Mat. Res. 106, 1770–1777. doi:10.1002/jbm.b.33984

PubMed Abstract | CrossRef Full Text | Google Scholar

Pashneh-Tala, S., Moorehead, R., and Claeyssens, F. (2020). Hybrid manufacturing strategies for tissue engineering scaffolds using methacrylate functionalised poly(glycerol sebacate). J. Biomater. Appl. 34, 1114–1130. doi:10.1177/0885328219898385

PubMed Abstract | CrossRef Full Text | Google Scholar

Pashneh-Tala, S., Owen, R., Bahmaee, H., Rekstyte, S., Malinauskas, M., and Claeyssens, F. (2018). Synthesis, characterization and 3D micro-structuring via 2-photon polymerization of poly(glycerol sebacate)-methacrylate-an elastomeric degradable polymer. Front. Phys. 6, 41. doi:10.3389/fphy.2018.00041

CrossRef Full Text | Google Scholar

Patel, A., Gaharwar, A. K., Iviglia, G., Zhang, H., Mukundan, S., Mihaila, S. M., et al. (2013). Highly elastomeric poly(glycerol sebacate)-co-poly(ethylene glycol) amphiphilic block copolymers. Biomaterials 34, 3970–3983. doi:10.1016/j.biomaterials.2013.01.045

PubMed Abstract | CrossRef Full Text | Google Scholar

Pereira, M. J. N., Ouyang, B., Sundback, C. A., Lang, N., Friehs, I., Mureli, S., et al. (2013). A highly tunable biocompatible and multifunctional biodegradable elastomer. Adv. Mat. 25, 1209–1215. doi:10.1002/adma.201203824

PubMed Abstract | CrossRef Full Text | Google Scholar

Perin, G. B., and Felisberti, M. I. (2020). Enzymatic synthesis of poly(glycerol sebacate): Kinetics, chain growth, and branching behavior. Macromolecules 53, 7925–7935. doi:10.1021/acs.macromol.0c01709

PubMed Abstract | CrossRef Full Text | Google Scholar

Piszko, P., Kryszak, B., Piszko, A., and Szustakiewicz, K. (2021). Brief review on poly(glycerol sebacate) as an emerging polyester in biomedical application: Structure, properties and modifications. Polim. Med. 51, 43–50. doi:10.17219/pim/139585

PubMed Abstract | CrossRef Full Text | Google Scholar

Piszko, P., Wlodarczyk, M., Zielinska, S., Gazinska, M., Plocinski, P., Rudnicka, K., et al. (2021). PGS/HAp Microporous composite scaffold obtained in the TIPS-TCL-SL method: An Innovation for bone tissue engineering. Int. J. Mol. Sci. 22, 8587. doi:10.3390/ijms22168587

PubMed Abstract | CrossRef Full Text | Google Scholar

Pomerantseva, I., Krebs, N., Hart, A., Neville, C. M., Huang, A. Y., and Sundback, C. A. (2009). Degradation behavior of poly(glycerol sebacate). J. Biomed. Mat. Res. A 91A, 1038–1047. doi:10.1002/jbm.a.32327

PubMed Abstract | CrossRef Full Text | Google Scholar

Quispe, C. a. G., Coronado, C. J. R., and Carvalho, J. (2013). a. Glycerol: Production, consumption, prices, characterization and new trends in combustion. Renew. Sustain. Energy Rev. 27, 475–493.

CrossRef Full Text | Google Scholar

Rai, R., Tallawi, M., Barbani, N., Frati, C., Madeddu, D., Cavalli, S., et al. (2013). Biomimetic poly(glycerol sebacate) (PGS) membranes for cardiac patch application. Mater. Sci. Eng. C 33, 3677–3687. doi:10.1016/j.msec.2013.04.058

PubMed Abstract | CrossRef Full Text | Google Scholar

Rai, R., Tallawi, M., Frati, C., Falco, A., Gervasi, A., Quaini, F., et al. (2015). Bioactive electrospun fibers of poly(glycerol sebacate) and poly(ε-caprolactone) for cardiac patch application. Adv. Healthc. Mat. 4, 2012–2025. doi:10.1002/adhm.201500154

PubMed Abstract | CrossRef Full Text | Google Scholar

Rai, R., Tallawi, M., Grigore, A., and Boccaccini, A. R. (2012). Synthesis, properties and biomedical applications of poly(glycerol sebacate) (PGS): A review. Prog. Polym. Sci. 37, 1051–1078. doi:10.1016/j.progpolymsci.2012.02.001

CrossRef Full Text | Google Scholar

Rai, R., Tallawi, M., Roether, J. A., Detsch, R., Barbani, N., Rosellini, E., et al. (2013). Sterilization effects on the physical properties and cytotoxicity of poly(glycerol sebacate). Mat. Lett. 105, 32–35. doi:10.1016/j.matlet.2013.04.024

CrossRef Full Text | Google Scholar

Rastegar, S., Mehdikhani, M., Bigham, A., Poorazizi, E., and Rafienia, M. (2021). Poly glycerol sebacate/polycaprolactone/carbon quantum dots fibrous scaffold as a multifunctional platform for cardiac tissue engineering. Mat. Chem. Phys. 266, 124543. doi:10.1016/j.matchemphys.2021.124543

CrossRef Full Text | Google Scholar

Ravichandran, R., Venugopal, J. R., Sundarrajan, S., Mukherjee, S., Sridhar, R., and Ramakrishna, S. (2012). Minimally invasive injectable short nanofibers of poly(glycerol sebacate) for cardiac tissue engineering. Nanotechnology 23, 385102. doi:10.1088/0957-4484/23/38/385102

PubMed Abstract | CrossRef Full Text | Google Scholar

Redenti, S., Neeley, W. L., Rompani, S., Saigal, S., Yang, J., Klassen, H., et al. (2009). Engineering retinal progenitor cell and scrollable poly(glycerol-sebacate) composites for expansion and subretinal transplantation. Biomaterials 30, 3405–3414. doi:10.1016/j.biomaterials.2009.02.046

PubMed Abstract | CrossRef Full Text | Google Scholar

Rekabgardan, M., Rahmani, M., Soleimani, M., HosSein Zadeh, S., Roozafzoon, R., Parandakh, A., et al. (2022). A Bilayered, electrospun poly(glycerol-sebacate)/polyurethane-polyurethane scaffold for engineering of endothelial Basement membrane. ASAIO J. 68, 123–132. doi:10.1097/mat.0000000000001423

PubMed Abstract | CrossRef Full Text | Google Scholar

Rezk, A. I., Kim, K.-S., and Kim, C. S. (2020). Poly(ε-Caprolactone)/Poly(Glycerol sebacate) composite nanofibers incorporating hydroxyapatite nanoparticles and simvastatin for bone tissue regeneration and drug delivery applications. Polym. (Basel). 12, 2667. doi:10.3390/polym12112667

PubMed Abstract | CrossRef Full Text | Google Scholar

Riaz, R., Abbas, S. R., and Iqbal, M. Synthesis (2022). Synthesis, rheological characterization, and proposed application of pre-polyglycerol sebacate as ultrasound contrast agent based on theoretical estimation. J. Appl. Polym. Sci. 139, 51963. doi:10.1002/app.51963

CrossRef Full Text | Google Scholar

Risley, B. B., Ding, X., Chen, Y., Miller, P. G., and Wang, Y. (2021). Citrate crosslinked poly(glycerol sebacate) with tunable elastomeric properties. Macromol. Biosci. 21, 2000301. doi:10.1002/mabi.202000301

PubMed Abstract | CrossRef Full Text | Google Scholar

Rosenbalm, T. N., Teruel, M., Day, C. S., Donati, G. L., Morykwas, M., Argenta, L., et al. (2016). Structural and mechanical characterization of bioresorbable, elastomeric nanocomposites from poly(glycerol sebacate)/nanohydroxyapatite for tissue transport applications. J. Biomed. Mat. Res. 104, 1366–1373. doi:10.1002/jbm.b.33467

PubMed Abstract | CrossRef Full Text | Google Scholar

Rostamian, M., Hosseini, H., Fakhri, V., Talouki, P. Y., Farahani, M., Gharehtzpeh, A. J., et al. (2022). Introducing a bio sorbent for removal of methylene blue dye based on flexible poly(glycerol sebacate)/chitosan/graphene oxide ecofriendly nanocomposites. Chemosphere 289, 133219. doi:10.1016/j.chemosphere.2021.133219

PubMed Abstract | CrossRef Full Text | Google Scholar

Rostamian, M., Kalaee, M. R., Dehkordi, S. R., Panahi-Sarmad, M., Tirgar, M., and Goodarzi, V. (2020). Design and characterization of poly(glycerol-sebacate)-co-poly(caprolactone) (PGS-co-PCL) and its nanocomposites as novel biomaterials: The promising candidate for soft tissue engineering. Eur. Polym. J. 138, 109985. doi:10.1016/j.eurpolymj.2020.109985

CrossRef Full Text | Google Scholar

Ruther, F., Roether, J. A., and Boccaccini, A. R. (2022). 3D printing of mechanically resistant poly (glycerol sebacate) (PGS)zein scaffolds for potential cardiac tissue engineering applications. Adv. Eng. Mat. 24, 2101768. doi:10.1002/adem.202101768

CrossRef Full Text | Google Scholar

Ruther, F., Zimmermann, A., Engel, F. B., and Boccaccini, A. R. (2020). Improvement of the layer adhesion of composite cardiac patches. Adv. Eng. Mat. 22, 1900986. doi:10.1002/adem.201900986

CrossRef Full Text | Google Scholar

Salehi, S., Czugala, M., Stafiej, P., Fathi, M., Bahners, T., Gutmann, J. S., et al. (2017). Poly (glycerol sebacate)-poly (ε-caprolactone) blend nanofibrous scaffold as intrinsic bio- and immunocompatible system for corneal repair. Acta Biomater. 50, 370–380. doi:10.1016/j.actbio.2017.01.013

PubMed Abstract | CrossRef Full Text | Google Scholar

Sales, V. L., Engelmayr, G. C., Johnson, J. A., Gao, J., Wang, Y., Sacks, M. S., et al. (2007). Protein Precoating of elastomeric tissue-engineering scaffolds increased Cellularity, enhanced Extracellular matrix protein production, and differentially Regulated the Phenotypes of circulating endothelial progenitor cells. Circulation 116, I55–I63. doi:10.1161/circulationaha.106.6806637

PubMed Abstract | CrossRef Full Text | Google Scholar

Saudi, A., Rafienia, M., Zargar Kharazi, A., Salehi, H., Zarrabi, A., and Karevan, M. (2019). Design and fabrication of poly (glycerol sebacate)-based fibers for neural tissue engineering: Synthesis, electrospinning, and characterization. Polym. Adv. Technol. 1, 1427–1440. doi:10.1002/pat.4575

CrossRef Full Text | Google Scholar

Saudi, A., Zebarjad, S. M., Salehi, H., Katoueizadeh, E., and Alizadeh, A. (2022). Assessing physicochemical, mechanical, and in vitro biological properties of polycaprolactone/poly(glycerol sebacate)/hydroxyapatite composite scaffold for nerve tissue engineering. Mat. Chem. Phys. 275, 125224. doi:10.1016/j.matchemphys.2021.125224

CrossRef Full Text | Google Scholar

Sencadas, V., Sadat, S., and Silva, D. M. (2020). Mechanical performance of elastomeric PGS scaffolds under dynamic conditions. J. Mech. Behav. Biomed. Mat. 102, 103474. doi:10.1016/j.jmbbm.2019.103474

PubMed Abstract | CrossRef Full Text | Google Scholar

Sencadas, V., Tawk, C., and Alici, G. (2020). Environmentally friendly and biodegradable Ultrasensitive Piezoresistive Sensors for Wearable electronics applications. ACS Appl. Mat. Interfaces 12, 8761–8772. doi:10.1021/acsami.9b21739

PubMed Abstract | CrossRef Full Text | Google Scholar

Sha, D., Wu, Z., Zhang, J., Ma, Y., Yang, Z., and Yuan, Y. (2021). Development of modified and multifunctional poly(glycerol sebacate) (PGS)-based biomaterials for biomedical applications. Eur. Polym. J. 161, 110830. doi:10.1016/j.eurpolymj.2021.110830

CrossRef Full Text | Google Scholar

Shi, M., Steck, J., Yang, X., Zhang, G., Yin, J., and Suo, Z. (2020). Cracks outrun erosion in degradable polymers. Extreme Mech. Lett. 40, 100978. doi:10.1016/j.eml.2020.100978

CrossRef Full Text | Google Scholar

Silva, J. C., Udangawa, R. N., Chen, J., Mancinelli, C. D., Garrudo, F. F., Mikael, P. E., et al. (2020). Kartogenin-loaded coaxial PGS/PCL aligned nanofibers for cartilage tissue engineering. Mater. Sci. Eng. C 107, 110291. doi:10.1016/j.msec.2019.110291

PubMed Abstract | CrossRef Full Text | Google Scholar

Singh, D., Harding, A. J., Albadawi, E., Boissonade, F. M., Haycock, J. W., and Claeyssens, F. (2018). Additive manufactured biodegradable poly(glycerol sebacate methacrylate) nerve guidance conduits. Acta Biomater. 78, 48–63. doi:10.1016/j.actbio.2018.07.055

PubMed Abstract | CrossRef Full Text | Google Scholar

Sivanesan, D., Verma, R. S., and Prasad, E. (2021). 5FU encapsulated polyglycerol sebacate nanoparticles as anti-cancer drug carriers. RSC Adv. 11, 18984–18993. doi:10.1039/d1ra01722e

PubMed Abstract | CrossRef Full Text | Google Scholar

Slavko, E., and Taylor, M. S. (2017). Catalyst-controlled polycondensation of glycerol with diacyl chlorides: Linear polyesters from a trifunctional monomer. Chem. Sci. 8, 7106–7111. doi:10.1039/c7sc01886j

PubMed Abstract | CrossRef Full Text | Google Scholar

Souza, M. T., Tansaz, S., Zanotto, E. D., and Boccaccini, A. R. (2017). Bioactive glass fiber-reinforced PGS matrix composites for cartilage regeneration. Materials 10, 83. doi:10.3390/ma10010083

PubMed Abstract | CrossRef Full Text | Google Scholar

Stowell, C. E. T., Li, X., Matsunaga, M. H., Cockreham, C. B., Kelly, K. M., Cheetham, J., et al. (2020). Resorbable vascular grafts show rapid cellularization and degradation in the ovine carotid. J. Tissue Eng. Regen. Med. 14, 1673–1684. doi:10.1002/term.3128

PubMed Abstract | CrossRef Full Text | Google Scholar

Sun, Z.-J., Chen, C., Sun, M. Z., Ai, C. H., Lu, X. L., Zheng, Y. F., et al. (2009). The application of poly (glycerol–sebacate) as biodegradable drug carrier. Biomaterials 30, 5209–5214. doi:10.1016/j.biomaterials.2009.06.007

PubMed Abstract | CrossRef Full Text | Google Scholar

Sun, Z.-J., Sun, B., Tao, R. B., Xie, X., Lu, X. L., and Dong, D. L. (2013). A poly(glycerol-sebacate-curcumin) polymer with potential use for brain gliomas. J. Biomed. Mat. Res. A 101A, 253–260. doi:10.1002/jbm.a.34319

PubMed Abstract | CrossRef Full Text | Google Scholar

Sundback, C. A., Shyu, J., Wang, Y., Faquin, W., Langer, R., Vacanti, J., et al. (2005). Biocompatibility analysis of poly(glycerol sebacate) as a nerve guide material. Biomaterials 26, 5454–5464. doi:10.1016/j.biomaterials.2005.02.004

PubMed Abstract | CrossRef Full Text | Google Scholar

Talebi, A., Labbaf, S., Atari, M., and Parhizkar, M. (2021). Polymeric nanocomposite structures based on functionalized graphene with tunable properties for nervous tissue replacement. ACS Biomater. Sci. Eng. 7, 4591–4601. doi:10.1021/acsbiomaterials.1c00744

PubMed Abstract | CrossRef Full Text | Google Scholar

Tallá Ferrer, C., Vilariño-Feltrer, G., Rizk, M., Sydow, H. G., and Vallés-Lluch, A. (2020). Nanocomposites based on poly(glycerol sebacate) with silica nanoparticles with potential application in dental tissue engineering. Int. J. Polym. Mater. Polym. Biomaterials 69, 761–772. doi:10.1080/00914037.2019.1616197

CrossRef Full Text | Google Scholar

Tallawi, M., Dippold, D., Rai, R., D'Atri, D., Roether, J., Schubert, D., et al. (2016). Novel PGS/PCL electrospun fiber mats with patterned topographical features for cardiac patch applications. Mater. Sci. Eng. C 69, 569–576. doi:10.1016/j.msec.2016.06.083

PubMed Abstract | CrossRef Full Text | Google Scholar

Tallawi, M., Zebrowski, D. C., Rai, R., Roether, J. A., Schubert, D. W., El Fray, M., et al. (2015). Poly(glycerol sebacate)/poly(butylene succinate-butylene dilinoleate) fibrous scaffolds for cardiac tissue engineering. Tissue Eng. Part C. Methods 21, 585–596. doi:10.1089/ten.tec.2014.0445

PubMed Abstract | CrossRef Full Text | Google Scholar

Tang, B. C., Yao, C. L., Xieh, K. Y., and Hong, S. G. (2017). Improvement of physical properties of poly(glycerol sebacate) by copolymerization with polyhydroxybutyrate-diols. J. Polym. Res. 24, 215. doi:10.1007/s10965-017-1371-8

CrossRef Full Text | Google Scholar

Tang, J., Zhang, Z., Song, Z., Chen, L., Hou, X., and Yao, K. (2006). Synthesis and characterization of elastic aliphatic polyesters from sebacic acid, glycol and glycerol. Eur. Polym. J. 42, 3360–3366. doi:10.1016/j.eurpolymj.2006.09.008

CrossRef Full Text | Google Scholar

Tevlek, A., Agacik, D. T., and Aydin, H. M. (2020). Stretchable poly(glycerol-sebacate)/β-tricalcium phosphate composites with shape recovery feature by extrusion. J. Appl. Polym. Sci. 137, 48689. doi:10.1002/app.48689

CrossRef Full Text | Google Scholar

Tevlek, A., Hosseinian, P., Ogutcu, C., Turk, M., and Aydin, H. M. (2017). Bi-layered constructs of poly(glycerol-sebacate)-β-tricalcium phosphate for bone-soft tissue interface applications. Mater. Sci. Eng. C 72, 316–324. doi:10.1016/j.msec.2016.11.082

PubMed Abstract | CrossRef Full Text | Google Scholar

Tevlek, A., Topuz, B., Akbay, E., and Aydin, H. M. (2022). Surface channel patterned and endothelialized poly(glycerol sebacate) based elastomers. J. Biomater. Appl. 37, 287–302. doi:10.1177/08853282221085798

PubMed Abstract | CrossRef Full Text | Google Scholar

Torabi, H., Mehdikhani, M., Varshosaz, J., and Shafiee, F. (2021). An innovative approach to fabricate a thermosensitive melatonin-loaded conductive pluronic/chitosan hydrogel for myocardial tissue engineering. J. Appl. Polym. Sci. 138. doi:10.1002/app.50327

CrossRef Full Text | Google Scholar

Touré, A. B. R., Mele, E., and Christie, J. K. (2020). Multi-layer scaffolds of poly(caprolactone), poly(glycerol sebacate) and bioactive Glasses manufactured by combined 3D printing and electrospinning. Nanomaterials 10, 626. doi:10.3390/nano10040626

PubMed Abstract | CrossRef Full Text | Google Scholar

Tsai, Y.-T., Chang, C.-W., and Yeh, Y.-C. (2020). Formation of highly elastomeric and property-tailorable poly(glycerol sebacate)- co -poly(ethylene glycol) hydrogels through thiol–norbornene photochemistry. Biomater. Sci. 8, 4728–4738. doi:10.1039/d0bm00632g

PubMed Abstract | CrossRef Full Text | Google Scholar

Uyama, H., Inada, K., and Kobayashi, S. (1999). Regioselective polymerization of divinyl sebacate and triols using lipase catalyst. Macromol. Rapid Commun. 174, 171–174. doi:10.1002/(sici)1521-3927(19990401)20:4<171:aid-marc171>3.0.co;2-2

CrossRef Full Text | Google Scholar

Uyama, H., Inada, K., and Kobayashi, S. (2001). Regioselectivity control in lipase-catalyzed polymerization of divinyl sebacate and triols. Macromol. Biosci. 1, 40–44. doi:10.1002/1616-5195(200101)1:13.3.CO;2-K

CrossRef Full Text | Google Scholar

Valerio, O., Misra, M., and Mohanty, A. K. (2018). Poly(glycerol- co -diacids) polyesters: From glycerol Biorefinery to sustainable engineering applications, A review. ACS Sustain. Chem. Eng. 6, 5681–5693. doi:10.1021/acssuschemeng.7b04837

CrossRef Full Text | Google Scholar

Varshosaz, J., Choopannejad, Z., Minaiyan, M., and Kharazi, A. Z. (2021). Rapid hemostasis by nanofibers of polyhydroxyethyl methacrylate/polyglycerol sebacic acid: An in vitro/in vivo study. J. Appl. Polym. Sci. 138, 49785. doi:10.1002/app.49785

CrossRef Full Text | Google Scholar

Vilariño-Feltrer, G., Muñoz-Santa, A., Conejero-García, Á., and Vallés-Lluch, A. (2020). The effect of salt fusion processing variables on structural, physicochemical and biological properties of poly(glycerol sebacate) scaffolds. Int. J. Polym. Mater. Polym. Biomaterials 69, 938–945. doi:10.1080/00914037.2019.1636247

CrossRef Full Text | Google Scholar

Vogt, L., Liverani, L., Roether, J. A., and Boccaccini, A. R. (2018). Electrospun zein fibers incorporating poly(glycerol sebacate) for soft tissue engineering. Nanomaterials 8, 150. doi:10.3390/nano8030150

PubMed Abstract | CrossRef Full Text | Google Scholar

Vogt, L., Rivera, L. R., Liverani, L., Piegat, A., El Fray, M., and Boccaccini, A. R. (2019). Poly(ε-caprolactone)/poly(glycerol sebacate) electrospun scaffolds for cardiac tissue engineering using benign solvents. Mater. Sci. Eng. C 103, 109712. doi:10.1016/j.msec.2019.04.091

PubMed Abstract | CrossRef Full Text | Google Scholar

Vogt, L., Ruther, F., Salehi, S., and Boccaccini, A. R. (2021). Poly(Glycerol sebacate) in biomedical applications—a review of the recent literature. Adv. Healthc. Mat. 10, 2002026. doi:10.1002/adhm.202002026

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, B., Ji, P., Ma, Y., Song, J., You, Z., and Chen, S. (2021). Bacterial cellulose nanofiber reinforced poly(glycerol-sebacate) biomimetic matrix for 3D cell culture. Cellulose 28, 8483–8492. doi:10.1007/s10570-021-04053-9

CrossRef Full Text | Google Scholar

Wang, L., Xu, K., Hou, X., Han, Y., Liu, S., Wiraja, C., et al. (2017). Fluorescent poly(glycerol- co -sebacate) acrylate nanoparticles for stem cell Labeling and Longitudinal Tracking. ACS Appl. Mat. Interfaces 9, 9528–9538. doi:10.1021/acsami.7b01203

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, M., Lei, D., Liu, Z., Chen, S., Sun, L., Lv, Z., et al. (2017). A poly(glycerol sebacate) based photo/thermo dual curable biodegradable and biocompatible polymer for biomedical applications. J. Biomaterials Sci. Polym. Ed. 28, 1728–1739. doi:10.1080/09205063.2017.1348927

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, S., Jeffries, E., Gao, J., Sun, L., You, Z., and Wang, Y. (2016). Polyester with Pendent Acetylcholine-mimicking Functionalities promotes neurite growth. ACS Appl. Mat. Interfaces 8, 9590–9599. doi:10.1021/acsami.5b12379

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, Y., Ameer, G. A., Sheppard, B. J., and Langer, R. (2002). A tough biodegradable elastomer. Nat. Biotechnol. 20, 602–606. doi:10.1038/nbt0602-602

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, Y., Kim, Y. M., and Langer, R. (2003). In vivo degradation characteristics of poly(glycerol sebacate). J. Biomed. Mat. Res. 66A, 192–197. doi:10.1002/jbm.a.10534

PubMed Abstract | CrossRef Full Text | Google Scholar

Wang, Z., Ma, Y., Wang, Y., Liu, Y., Chen, K., Wu, Z., et al. (2018). Urethane-based low-temperature curing, highly-customized and multifunctional poly(glycerol sebacate)-co-poly(ethylene glycol) copolymers. Acta Biomater. 71, 279–292. doi:10.1016/j.actbio.2018.03.011

PubMed Abstract | CrossRef Full Text | Google Scholar

Wilson, R., Divakaran, A. V., Varyambath, A., Kumaran, A., Sivaram, S., et al. (2018). Poly(glycerol sebacate)-based polyester-Polyether copolymers and their semi-Interpenetrated networks with thermoplastic poly(ester-ether) elastomers: Preparation and properties. ACS Omega 3, 18714–18723. doi:10.1021/acsomega.8b02451

PubMed Abstract | CrossRef Full Text | Google Scholar

Wrzecionek, M., Howis, J., Marek, P. H., Ruśkowski, P., and Gadomska-Gajadhur, A. (2021). The catalyst-free polytransesterification for obtaining linear PGS optimized with use of 22 factorial design. Chem. Process Eng. - Inz. Chem. i Proces. 42, 43–52.

Google Scholar

Wu, H.-J., Hu, M.-H., Tuan-Mu, H.-Y., and Hu, J.-J. (2019). Preparation of aligned poly(glycerol sebacate) fibrous membranes for anisotropic tissue engineering. Mater. Sci. Eng. C 100, 30–37. doi:10.1016/j.msec.2019.02.098

PubMed Abstract | CrossRef Full Text | Google Scholar

Wu, T., Frydrych, M., O’Kelly, K., and Chen, B. (2014). Poly(glycerol sebacate urethane)–cellulose nanocomposites with water-Active shape-memory effects. Biomacromolecules 15, 2663–2671. doi:10.1021/bm500507z

PubMed Abstract | CrossRef Full Text | Google Scholar

Wu, W., Jia, S., Chen, W., Liu, X., and Zhang, S. (2019). Fast degrading elastomer stented fascia remodels into tough and vascularized construct for tracheal regeneration. Mater. Sci. Eng. C 101, 1–14. doi:10.1016/j.msec.2019.02.108

PubMed Abstract | CrossRef Full Text | Google Scholar

Wu, Y., Wang, L., Guo, B., and X Ma, P. (2014). Injectable biodegradable hydrogels and microgels based on methacrylated poly(ethylene glycol)-co-poly(glycerol sebacate) multi-block copolymers: Synthesis, characterization, and cell encapsulation. J. Mat. Chem. B 2, 3674. doi:10.1039/c3tb21716g

PubMed Abstract | CrossRef Full Text | Google Scholar

Wu, Y., Wang, L., Zhao, X., Hou, S., Guo, B., and Ma, P. X. (2016). Self-healing supramolecular bioelastomers with shape memory property as a multifunctional platform for biomedical applications via modular assembly. Biomaterials 104, 18–31. doi:10.1016/j.biomaterials.2016.07.011

PubMed Abstract | CrossRef Full Text | Google Scholar

Wu, Z., Jin, K., Wang, L., and Fan, Y. (2021). A review: Optimization for poly(glycerol sebacate) and fabrication techniques for its Centered scaffolds. Macromol. Biosci. 21, 2100022. doi:10.1002/mabi.202100022

PubMed Abstract | CrossRef Full Text | Google Scholar

Wyatt, V. T., Strahan, G. D., Wyatt, V. T., and Strahan, G. D. (2012). Degree of branching in hyperbranched poly(glycerol-co-diacid)s synthesized in toluene. Polym. (Basel) 4, 396–407. doi:10.3390/polym4010396

CrossRef Full Text | Google Scholar

Xiao, B., Yang, W., Lei, D., Huang, J., Yin, Y., Zhu, Y., et al. (2019). PGS scaffolds promote the In vivo Survival and Directional differentiation of bone marrow mesenchymal stem cells restoring the morphology and function of wounded rat uterus. Adv. Healthc. Mat. 8, 1801455. doi:10.1002/adhm.201801455

PubMed Abstract | CrossRef Full Text | Google Scholar

Xu, B., Li, Y., Zhu, C., Cook, W. D., Forsythe, J., and Chen, Q. (2015). Fabrication, mechanical properties and cytocompatibility of elastomeric nanofibrous mats of poly(glycerol sebacate). Eur. Polym. J. 64, 79–92. doi:10.1016/j.eurpolymj.2014.12.008

CrossRef Full Text | Google Scholar

Xuan, H., Hu, H., Geng, C., Song, J., Shen, Y., Lei, D., et al. (2020). Biofunctionalized chondrogenic shape-memory ternary scaffolds for efficient cell-free cartilage regeneration. Acta Biomater. 105, 97–110. doi:10.1016/j.actbio.2020.01.015

PubMed Abstract | CrossRef Full Text | Google Scholar

Yan, Y., Sencadas, V., Jin, T., Huang, X., Lie, W., Wei, D., et al. (2018). Effect of multi-walled carbon nanotubes on the cross-linking density of the poly(glycerol sebacate) elastomeric nanocomposites. J. Colloid Interface Sci. 521, 24–32. doi:10.1016/j.jcis.2018.03.015

PubMed Abstract | CrossRef Full Text | Google Scholar

Yang, B., Lv, W., and Deng, Y. (2017). Drug loaded poly(glycerol sebacate) as a local drug delivery system for the treatment of periodontal disease. RSC Adv. 7, 37426–37435. doi:10.1039/c7ra02796f

CrossRef Full Text | Google Scholar

Yang, K., Zhang, J., Ma, X., Ma, Y., Kan, C., Ma, H., et al. (2015). β-Tricalcium phosphate/poly(glycerol sebacate) scaffolds with robust mechanical property for bone tissue engineering. Mater. Sci. Eng. C 56, 37–47. doi:10.1016/j.msec.2015.05.083

PubMed Abstract | CrossRef Full Text | Google Scholar

Yang, Y., Yu, Y., Zhang, Y., Liu, C., Shi, W., and Li, Q. (2011). Lipase/esterase-catalyzed ring-opening polymerization : A green polyester synthesis technique. Process Biochem. 46, 1900–1908. doi:10.1016/j.procbio.2011.07.016

CrossRef Full Text | Google Scholar

Yeh, Y.-C., Highley, C. B., Ouyang, L., and Burdick, J. A. (2016). 3D printing of photocurable poly(glycerol sebacate) elastomers. Biofabrication 8, 045004. doi:10.1088/1758-5090/8/4/045004

PubMed Abstract | CrossRef Full Text | Google Scholar

Yeh, Y.-C., Ouyang, L., Highley, C. B., and Burdick, J. A. (2017). Norbornene-modified poly(glycerol sebacate) as a photocurable and biodegradable elastomer. Polym. Chem. 8, 5091–5099. doi:10.1039/c7py00323d

CrossRef Full Text | Google Scholar

Yi, F., and La Van, D. A. (2008). Poly(glycerol sebacate) nanofiber scaffolds by core/shell electrospinning. Macromol. Biosci. 8, 803–806. doi:10.1002/mabi.200800041

PubMed Abstract | CrossRef Full Text | Google Scholar

You, Z., Cao, H., Gao, J., Shin, P. H., Day, B. W., and Wang, Y. (2010). A functionalizable polyester with free hydroxyl groups and tunable physiochemical and biological properties. Biomaterials 31, 3129–3138. doi:10.1016/j.biomaterials.2010.01.023

PubMed Abstract | CrossRef Full Text | Google Scholar

You, Z. R., Hu, M. H., Tuan-Mu, H. Y., and Hu, J. J. (2016). Fabrication of poly(glycerol sebacate) fibrous membranes by coaxial electrospinning: Influence of shell and core solutions. J. Mech. Behav. Biomed. Mat. 63, 220–231. doi:10.1016/j.jmbbm.2016.06.022

PubMed Abstract | CrossRef Full Text | Google Scholar

Yu, Y., Wu, D., Liu, C., Zhao, Z., Yang, Y., and Li, Q. (2012). Lipase/esterase-catalyzed synthesis of aliphatic polyesters via polycondensation: A review. Process Biochem. 47, 1027–1036. doi:10.1016/j.procbio.2012.04.006

CrossRef Full Text | Google Scholar

Zaky, S. H., Lee, K., Gao, J., Jensen, A., Verdelis, K., Wang, Y., et al. (2017). Poly (glycerol sebacate) elastomer supports bone regeneration by its mechanical properties being closer to osteoid tissue rather than to mature bone. Acta Biomater. 54, 95–106. doi:10.1016/j.actbio.2017.01.053

PubMed Abstract | CrossRef Full Text | Google Scholar

Zanjanizadeh Ezazi, N., Ajdary, R., Correia, A., Makila, E., Salonen, J., Kemell, M., et al. (2020). Fabrication and characterization of drug-loaded conductive poly(glycerol sebacate)/Nanoparticle-based composite patch for myocardial Infarction applications. ACS Appl. Mat. Interfaces 12, 6899–6909. doi:10.1021/acsami.9b21066

PubMed Abstract | CrossRef Full Text | Google Scholar

Zbinden, J. C., Blum, K. M., Berman, A. G., Ramachandra, A. B., Szafron, J. M., Kerr, K. E., et al. (2020). Tissue-engineered vascular grafts: Effects of Braiding parameters on tissue engineered vascular graft development. Adv. Healthc. Mat. 9, 2070086. doi:10.1002/adhm.202070086

PubMed Abstract | CrossRef Full Text | Google Scholar

Zhang, C., Wen, T. H., Razak, K. A., Lin, J., Xu, C., Seo, C., et al. (2020). Magnesium-based biodegradable microelectrodes for neural recording. Mater. Sci. Eng. C 110, 110614. doi:10.1016/j.msec.2019.110614

PubMed Abstract | CrossRef Full Text | Google Scholar

Zhang, J., Shi, H., Wu, D., Xing, Z., and Zhang, A. (2014). Recent developments in lipase-catalyzed synthesis of polymeric materials. Process Biochem. 49, 797–806. doi:10.1016/j.procbio.2014.02.006

CrossRef Full Text | Google Scholar

Zhang, X., Jia, C., Qiao, X., Liu, T., and Sun, K. (2016). Porous poly(glycerol sebacate) (PGS) elastomer scaffolds for skin tissue engineering. Polym. Test. 54, 118–125. doi:10.1016/j.polymertesting.2016.07.006

CrossRef Full Text | Google Scholar

Zhang, X., Jia, C., Qiao, X., Liu, T., and Sun, K. (2017). Silk fibroin microfibers and chitosan modified poly (glycerol sebacate) composite scaffolds for skin tissue engineering. Polym. Test. 62, 88–95. doi:10.1016/j.polymertesting.2017.06.012

CrossRef Full Text | Google Scholar

Zhang, Y., Liu, Y., Jiang, Z., Wang, J., Xu, Z., Meng, K., et al. (2021). Poly(glyceryl sebacate)/silk fibroin small-diameter artificial blood vessels with good elasticity and compliance. Smart Mat. Med. 2, 74–86. doi:10.1016/j.smaim.2021.01.001

CrossRef Full Text | Google Scholar

Zhang, Y., Spinella, S., Xie, W., Cai, J., Yang, Y., Wang, Y. Z., et al. (2013). Polymeric triglyceride analogs prepared by enzyme-catalyzed condensation polymerization. Eur. Polym. J. 49, 793–803. doi:10.1016/j.eurpolymj.2012.11.011

CrossRef Full Text | Google Scholar

Zhao, X., Wu, H., Guo, B., Dong, R., Qiu, Y., and Ma, P. X. (2017). Antibacterial anti-oxidant electroactive injectable hydrogel as self-healing wound dressing with hemostasis and adhesiveness for cutaneous wound healing. Biomaterials 122, 34–47. doi:10.1016/j.biomaterials.2017.01.011

PubMed Abstract | CrossRef Full Text | Google Scholar

Zhou, L., He, H., Jiang, C., and He, S. (2015). Preparation and characterization of poly(glycerol sebacate)/cellulose nanocrystals elastomeric composites. J. Appl. Polym. Sci. 132, 27. doi:10.1002/app.42196

CrossRef Full Text | Google Scholar

Zhu, C., Rodda, A. E., Truong, V. X., Shi, Y., Zhou, K., Haynes, J. M., et al. (2018). Increased Cardiomyocyte Alignment and intracellular calcium Transients using Micropatterned and drug-releasing poly(glycerol sebacate) elastomers. ACS Biomater. Sci. Eng. 4, 2494–2504. doi:10.1021/acsbiomaterials.8b00084

PubMed Abstract | CrossRef Full Text | Google Scholar

Zulkifli, Z., Tan, J. J., Ku Marsilla, K. I., Rusli, A., Abdullah, M. K., Shuib, R. K., et al. (2022). Shape memory poly (glycerol sebacate)based electrospun fiber scaffolds for tissue engineering applications: A review. J. Appl. Polym. Sci. 139, 52272. doi:10.1002/app.52272

CrossRef Full Text | Google Scholar

Keywords: poly(glycerol sebacate) (PGS), microwave-assisted synthesis, enzymatic synthesis, polycondensation synthesis, PGS-based materials

Citation: Godinho B, Gama N and Ferreira A (2022) Different methods of synthesizing poly(glycerol sebacate) (PGS): A review. Front. Bioeng. Biotechnol. 10:1033827. doi: 10.3389/fbioe.2022.1033827

Received: 01 September 2022; Accepted: 10 November 2022;
Published: 30 November 2022.

Edited by:

Verónica de Zea Bermudez, University of Trás-os-Montes and Alto Douro, Portugal

Reviewed by:

Atakan Tevlek, Middle East Technical University, Turkey
Bartłomiej Kryszak, Wrocław University of Science and Technology, Poland

Copyright © 2022 Godinho, Gama and Ferreira. This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.

*Correspondence: Artur Ferreira, artur.ferreira@ua.pt

Disclaimer: All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.