Skip to main content

ORIGINAL RESEARCH article

Front. Chem., 28 February 2019
Sec. Green and Sustainable Chemistry
This article is part of the Research Topic Ionic Liquids: Properties and Applications View all 30 articles

Non-halogenated Ionic Liquid Dramatically Enhances Tribological Performance of Biodegradable Oils

  • 1Machine Design, KTH Royal Institute of Technology, Stockholm, Sweden
  • 2Department of Chemistry, KTH Royal Institute of Technology, Stockholm, Sweden
  • 3Chemistry of Interfaces, Luleå University of Technology, Luleå, Sweden
  • 4Surfaces, Processes and Formulation, RISE Research Institutes of Sweden, Stockholm, Sweden
  • 5Department of Electrical Energy, Metals, Mechanical Constructions and Systems, Ghent University, Ghent, Belgium

It is demonstrated that a phosphonium orthoborate ionic liquid may serve as a wear reducing additive in biodegradable oils at steel-steel surfaces in the boundary lubrication regime. Tribological tests were performed in a ball-on-three plate configuration. A set of surface characterization techniques—SEM/EDS, FIB and white light interferometry were used to characterize surfaces following the tribotests and to observe the formation of any tribofilms. 11B NMR was used to follow changes in the composition of the ionic-liquid-oil blends and to identify boron-containing decomposition products after the tribotests. The ionic liquid reduces the wear of steel surfaces by up to 92% compared to the neat oil at 90°C; it is shown that the reduction in wear can be correlated with the formation of boron enriched patches in the boundary films.

Introduction

The mounting pressure for a transition from mineral to biodegradable oils in many industrial applications implies a number of technological challenges. One of them is to identify the next generation of wear reducing additives. Most current anti-wear additives, such as zinc dialkyldithiophosphates (ZDDP) and tricresyl phosphates (TCP), were developed in late 1940s for use with mineral oils. Despite their good wear reducing properties for lubricated steel-steel contacts (Martin, 1999; Fujita and Spikes, 2004), there are environmental concerns regarding the use of ZDDP and TCP. ZDDP containing formulations tend to form zinc and phosphorus rich ashes in internal combustion engines, which poison catalysts and consequently worsen the exhaust quality (Xie et al., 2016). Similar problems are related to the use of TCP, which promotes formation of toxic species upon its decomposition at lubrication contacts at elevated temperatures (Michaelis, 2011; Ramsden, 2013), and it is intrinsically toxic in its pure form (Goldstein et al., 1988). Moreover, the wear reducing performance of these additives in biodegradable oils is rather moderate according to four-ball configuration mechanical tests for steel-steel contacts: it has been reported that vegetable oils with ZDDP additives result in only up to 13% reduction of the wear scar diameter when compared with the neat oil (Mahipal et al., 2014). Choi et al. have studied the performance of TCP in vegetable oils and reported up to 30% reduction in the wear scar diameters when compared to the neat oils (Choi et al., 1997).

A range of alternative additive approaches have been examined, including other phosphorus compounds (Johnson and Hils, 2013) and nanoparticles (Shahnazar et al., 2016). Hybrid approaches have also been used, for example when combining diamond nanoparticles with phosphoesters (Acharya et al., 2018). Another promising avenue to address the challenge is the use of ionic liquids (ILs). Knowledge of ILs in lubrication is rapidly expanding and the growing number of publications on ILs as neat lubricants or additives to oils (Zhou and Qu, 2017) is clear evidence of this. Ionic liquids also provide the opportunity to control the friction properties via the use of electric fields due to their ionic nature (Sweeney et al., 2012; Cooper et al., 2016)—so called tribotronics (Glavatskih and Höglund, 2008). However, a significant fraction of the published work is on halogenated ILs, which for historical reasons are commercially available, but are of limited interest to industry (Totten et al., 2003) due to environmental and health reasons. The “rear-view mirror” approach to the development of the ionic liquids field in general—that is to say the vicious circle of ionic liquid selection based on previous studies for benchmarking purposes—was highlighted at the recent Faraday Discussions on Ionic Liquids, and indeed formed the basis of the closing address (Jessop, 2018). A further key element concerning the “sustainability” of ionic liquids was a salutary reminder that one cannot consider the relative merits of ILs vs. their conventional counterparts in their application alone, but that the environmental impact of their manufacture should also be compared. Successful candidates for industrial applications in the field of tribology (the study of friction, lubrication, and wear) need to be non-halogenated ILs engineered to meet the requirements of the lubrication industry (Shah et al., 2011). The choice and structure of cations and anions are dictated by the application specifics such as the materials to be lubricated, the contact geometry and pressure, as well as the speed, ambient conditions and type of movement (sliding/rolling, reciprocating/continuous). An example of an exception to the use of halogenated ILs is the work of Kronberger et al. They investigated tribological performance of a number of neat ILs and IL solutions in glycerol (Kronberger et al., 2012) using sulfur based anions [sulfates (Pejakovic et al., 2012) and sulphonates] and nitrogen based cations (n-alkylammonium, cholines, pyrrolidinium). In some cases both friction and wear were reduced compared to neat glycerol, with neat ILs and solutions performing similarly. XPS analysis of the worn surfaces suggest that the performance is enhanced by formation of iron sulfide tribolayers on the metal surfaces. The same authors have also pointed out that miscibility of an IL with a carrier fluid is crucial for their deployment (Kronberger et al., 2014).

Xie et al. have recently compared ZDDP with phosphonium based ionic liquids (ILs) and concluded that ILs have less impact on the functionality of the catalysts (Xie et al., 2016). Phosphonium cations are known for their wear reducing performance and the anti-wear boundary films produced on the lubricated surfaces have been shown to contain phosphorus (Westerholt et al., 2015). A corrosion inhibition effect of phosphonium cations has also been observed (Kondo et al., 2012). It has also been reported that ILs containing phosphorus in both anion and cation are efficient anti-wear additives to non-polar oils (Qu et al., 2015). An enhancement in the anti-wear performance of phosphonium ILs as additives to a mineral oil was achieved by adding a borate ester (Sharma et al., 2016) to the oil blend. Boron is known to form friction and wear reducing compounds in lubricated contacts (Shah et al., 2013) and ILs consisting of phosphorus and boron based ions have thus been the target of synthesis (Shah et al., 2011). Such ILs have formed the focus of a range of nanotribology and model studies (Li et al., 2016; Cooper et al., 2017; Cowie et al., 2017) confirming this promise. In this work, boron and phosphorus are incorporated in a single IL, as the anion and cation respectively, trihexyltetradecylphosphonium bis(mandelato)borate (P-BMB), which is then used as an additive to biodegradable oils. The goal is to study how the IL additive improves oil lubrication performance on steel surfaces, and to relate this to the additive properties, and to any antiwear films generated on the surfaces.

Materials and Methods

P-BMB was synthesized and characterized as previously described (Shah et al., 2011). The higher polarity of biodegradable oils compared to conventional mineral oils increases their affinity for the surface and may also have implications for the transport properties of the IL. Two representative biodegradable oils were selected for the tests. Oil soluble polyalkylene glycol (OPAG), UCON OSP46 (Dow Chemicals inherently biodegradable; more than 35 % during 28 days), and a monoester (ME), Estisol 240 (Estichem, readily biodegradable; more than 60% during 28 days), were used in the lubrication tests. The exact chemical structure of OPAG is undisclosed which underlines some of the challenges of performing relevant tribological research from a chemical perspective. Estisol 240 is a C8-C6 monoester, hexyl-octanoate with a structure shown in Figure 1 and has a non-polarity index of 32. To ensure homogeneous blends, the blends were ultrasonicated for at least 60 min at 50°C. Table S1 shows viscosities of IL, oils and the blends of oils with IL. Viscosities were measured with a HR-2 rheometer, TA Instruments.

FIGURE 1
www.frontiersin.org

Figure 1. The structure of the C8-C6 monoester, hexyl-octanoate, denoted in the text as ME. Red, O; gray, C; white, H.

Solubility Tests of Ionic Liquids

Several IL-oil mixtures were prepared with IL concentrations varied within 0–20 wt.%. After having been thoroughly mixed, the samples were centrifuged at a speed of 6,500 rpm. An equal amount of supernatant was then carefully taken from all mixtures, centrifuged and placed into separate NMR tubes. Quantitative 31P and 1H NMR were run on the resultant samples of the ME and OPAG blends. Obtained NMR spectra were processed: “0” and “1” order phase corrections were applied; the baseline was corrected using a first order polynomial correction. After that spectral regions corresponding to the IL liquid were integrated. The resultant integral values were normalized according to the integral value obtained from the sample with an IL concentration of 1 wt%. The initial concentrations were determined from the actual IL and oil weights used before the centrifugation.

Test Procedure

The same rheometer that was used for measuring lubricant viscosities was utilized for the lubrication tests. A set-up with a ball-on-three-plates configuration as shown in Figure S1 was installed. (This setup allows high contact pressures, continuous sliding—typical for lubricated contacts, faster lubricant consumption and the plates are compatible with SEM analysis). The ball was pressed against the plates with an initial maximum Hertzian contact pressure of 1.11 GPa. This load, corresponding to 21 N per contact, was selected to place the contact in the boundary regime, for which this is an appropriate pressure; similar contact pressures have been used in related publications. 1.13 GPa was employed to study neat IL lubrication of steel (Garcia et al., 2014), while 1.0 GPa maximum pressure was used in two studies of IL as additives to glycerol (Kronberger et al., 2012; Pejakovic et al., 2012; Garcia et al., 2014). Each test was run with a sliding speed of 0.2 ms−1 for a sliding distance of 2000 m. (This sliding speed and distance provide a balance between experimental time and a suitable degree of wear). Normal and friction forces were recorded with an acquisition frequency of 1 Hz. Friction coefficients during 500 m of sliding were then averaged. Oil bath temperature, set to 90°C, was regulated by a Peltier element. A test run required 1.2 ml of lubricant and was repeated 4 times. Relative humidity, measured during the tests, was 40 ± 5% at an ambient temperature of 22 ± 2°C. The ⊘12.7 mm steel balls (AISI 52100, Rotera Kullager AB, Täby, Sweden), used in the lubrication tests, had a measured roughness of Ra = 0.074 ± 0.006 μm and a hardness of 60–67 HRC (Rockwell Hardness, according to the supplier). The mating surface, AISI 52100 steel plates, had a measured hardness of 64 HRC and roughness of Ra = 0.142 ± 0.028 μm. The roughness was measured with a Taylor Hobsen PGI 800 Profilometer from Talysurf. The hardness was determined by measuring indents with an optical microscope from Nikon (MM-60/L3). The plates were cut from the rolling bearing discs and had the following dimensions: 3 mm in thickness, 6 mm in width and 7 mm in length. Before each test, balls and plates were cleaned in several steps. First, they were ultrasonicated in acetone for 30 min and then dried under a dry air stream. Next, they were ultrasonicated in isopropanol for 30 min and finally dried by dry air stream again. After the tribological experiments balls and plates were rinsed with ethanol and ultrasonicated twice (30 min each time), using fresh heptane each time. Then they were dried under a dry air flow and placed in a vacuum oven for 3 days at 50°C.

Wear, Interfacial Film, and Oil Analysis

The wear volume of the plates was measured by using a contact profilometer (Taylor Hobson PGI800) and an optical profiler (Zygo7300). The average wear volume Wv was calculated for each set of three plates and used to obtain the wear coefficient:

k=Wv/(FN×s),    (1)

where FN is the normal contact force on a single plate and s is sliding distance (Archard, 1953).

A Scanning Electron Microscope (SEM), JEOL 7800F, was employed to take images of the wear tracks at a beam energy of 10 kV. Distributions of chemical elements for selected points inside and outside the wear tracks were obtained by using an Energy Dispersive X-ray Spectroscopy (EDS), Bruker Quantax system.

A focused ion beam (FIB-SEM FEI NOVA 600) was used to create cross section cuts through the boundary film. Prior to each cut EDS spectra were recorded with 10 kV, followed by a deposition of a thin layer (~500 nm) of platinum on top of the investigated area (100 pA current, 30 kV voltage). Thereafter, the focused ion beam with a beam current of 3 nA and 30 kV voltage was utilized to create a wedge cut-out with a maximum depth of 4 μm at the edge of cross section. SEM images of the cut-outs were recorded with a 5 keV beam voltage.

11B NMR spectra of the oil blends before and after the lubrication tests were recorded at 160.5 MHz on a Bruker Avance III NMR spectrometer. A standard Broad Band probe from Bruker was used. Spectral width was set to 64 kHz and all NMR measurements were performed at 60°C. A 50 Hz exponential filter was applied to all spectra to reduce the noise level.

Results and Discussion

The normalized spectral integral values obtained for the blends prepared at room temperature are shown in Figure 2. The IL NMR integral values (corresponding to the amount of IL in the supernatants) for the ME blends are proportional to the initial concentrations of IL in a mixture. For the OPAG blends, a plateau of the NMR integral values is observed for the initial concentrations higher than 5 wt%. Addition of IL above this concentration to OPAG resulted in the precipitation of the added IL during the centrifugation stage. It is thus concluded that the IL is soluble in ME within the concentration range studied, whereas it has a limited solubility (up to 5 wt% at RT) in OPAG.

FIGURE 2
www.frontiersin.org

Figure 2. IL NMR integral value for supernatants of centrifuged mixtures as a function of the initial concentration. Circles are for 31P NMR and squares for 1H NMR. Solid lines are linear fits to the low-concentration experimental data.

The self-diffusion coefficients of the ions of the IL in oils were approximately one order of magnitude higher relative to their values in neat IL. Thus, the distribution of IL in the ME is considered stable and homogeneous and no liquid droplets exist.

Blends of 5 wt% IL with ME and OPAG were thus used for the lubrication tests (the concentrations of phosphorus and boron in the blends were 1,948 and 680 ppm, respectively). The results for all samples are shown in Figure 3. In the beginning of each test the running-in process resulted in a somewhat larger variation of the coefficient of friction. This variation decreased with time in all cases. However, for ME + IL more unstable friction returned toward the end of the test. Particularly after running-in it is clear that the OPAG+IL friction coefficients are uniformly lower than for OPAG, by ~10% The full data sets are shown in Figure S2. The fact that the friction coefficient values are similar, despite a 6-fold difference in viscosity between ME and OPAG samples at 90°C strongly indicates that the contact indeed operates in the targeted boundary lubrication regime, as opposed to “full film lubrication,” whereby a liquid film separates the surfaces. Since hydrodynamic effects are insignificant in boundary lubrication, it is concluded that surface protection is achieved through the interactions of oil molecules and additives with the lubricated surfaces.

FIGURE 3
www.frontiersin.org

Figure 3. Average friction coefficients over a sliding distance of 2,000 m. The data is divided into four intervals of the sliding distance to allow any distance or time dependent phenomena to be observed.

Monoesters are recognized as surface active compounds and are often used as friction modifiers with an anti-wear functionality (Spikes, 2015). Consequently, in these experiments neat ME provided ~5 times lower wear compared to OPAG. Similar trends for ME and polyglycols have previously been reported (Chen et al., 2009). The wear coefficients are presented in Figure 4. It can be seen that addition of IL resulted in significantly lower wear. The reduction was much larger (92%) for the OPAG/IL blend, reflecting the fact that OPAG has poorer intrinsic wear protection than ME. Optical images of the wear scars are shown in Figure 5. The wear scars attained with the neat oils are deep and are of a non-circular shape (see the ESI for details). Compared to the neat oils, the blends with IL produced much smaller and shallower wear scars. Scratches from the manufacturing process (polishing) were still visible on the plate surfaces after the tests. The depth of the scratches was similar to the wear scar depth for the oil/IL blends, emphasizing the mildness of the wear.

FIGURE 4
www.frontiersin.org

Figure 4. Wear coefficients for the plates lubricated by ME, OPAG and their blends with IL. Note that the axis for OPAG has been broken since the wear for the neat oil was much larger.

FIGURE 5
www.frontiersin.org

Figure 5. Optical images (1 × 1 mm) of the wear scars for (A) ME, (B) ME + IL, (C) OPAG, (D) OPAG + IL.

Biodegradable oils are designed to degrade if they leak into the environment but to remain stable in the lubrication system. However, due to high thermo-mechanical stresses in the lubricated interface, the oil may degrade in the contact producing compounds that can also be reactive toward ions, thus accelerating consumption of the IL and shortening lubricant service life. Note that reactivity can also have a positive effect if it contributes to the formation of stable, so called “antiwear” films on the surfaces in contact. Consumption of the IL in the blends was studied with NMR spectroscopy. The 11B NMR spectra of ME/IL and OPAG/IL blends taken before and after the lubrication tests were compared. The spectra before the tests showed a single resonance line, Figure 6, corresponding to the neat IL but this changed after the tests. Additional spectral lines appeared, indicating the orthoborate anion reacting to yield boron in a new chemical environment. The overall signal intensity (obtained by integration between −100 and 100 ppm) also decreased, relative to the initial (before the lubrication tests) situation. Those relative values are shown in percent in Figure 6. This finding indicates a depletion of soluble boron-containing (including the original orthoborate anions) species from the oil blends during the lubrication tests.

FIGURE 6
www.frontiersin.org

Figure 6. 11B NMR spectra and changes in the relative values of the spectral integral intensities for the ME + IL (A,B) and OPAG + IL (C,D blends). Intensities of the spectra recorded after the lubrication tests are amplified.

This effect is particularly strong for the ME blend where, in addition, hardly any of the boron-containing solutes are in the form of the original orthoborate species (as indicated by the near disappearance of the original resonance line at ca. 11 ppm). For the OPAG blend, neither the depletion nor the chemical reaction is as pronounced. Since the amount of boron in the oil blends decreased during the lubrication tests, it can be assumed that boron accumulated in the boundary films.

To investigate the veracity of this assumption, both the unworn and worn steel surfaces were analyzed using SEM-EDS. SEM images (insets in Figures 7, 8) revealed a patchy boundary film structure inside the wear track for both oil blends. The patches appeared to be larger in the case of OPAG/IL compared to the ME/IL blend. EDS spectra were recorded at a number of points located within the wear scar to probe the elemental composition of the patches. Reference EDS spectra were recorded at points located on the unworn surface outside the wear scar. Point positions are marked by numbers in the insets in Figures 7, 8. Spectra for the balls are not shown as no phosphorus or boron were detected in the wear scars on the ball surfaces. This is reasonable considering the less severe tribological conditions experienced by the ball surface due to the shorter contact time (see Figure S1).

FIGURE 7
www.frontiersin.org

Figure 7. EDS spectra for ME/IL obtained at several points as shown in the inserts. Spectra color codes are for different points: 1—red, 2—blue, 3—green, 4—black. The brown dashed line is for the unworn surface.

FIGURE 8
www.frontiersin.org

Figure 8. EDS spectra for OPAG/IL obtained at several points as shown in the inserts. Spectra color codes are for different points: 1—red, 2—blue, 3—green, 4—black. The brown dashed line is for the unworn surface.

The unworn plate surface contained iron, carbon, oxygen and traces of aluminum. Aluminum originates from the grinding and polishing process. Almost no aluminum was detected inside the wear scar, indicating that it was located within the very top surface layer and was removed by rubbing during the lubrication tests. The worn surfaces also showed an increased amount of oxygen and a decreased amount of iron. The lower intensity of the iron peak indicates that the boundary film was formed on top of the metal surface during the rubbing process. EDS spectra for a majority of the points taken in the oil/IL sample boundary films, formed by the oil/IL blends, showed the presence of both boron and phosphorus. The presence of boron enriched patches and the reduced boron concentration seen by 11B NMR appears to confirm that boron in the boundary films originated from the IL “consumed” during the lubrication tests.

It should be remembered however, that physically adsorbed IL at the lubricated surface can also contribute to the observations. The mechanism of boron mobility toward the lubricated surfaces and its surface activity includes a combination of processes. Since lubrication of steel can result in a locally positive surface charge (exo-electron emission; Nakayama et al., 1992), anions will consequently be preferentially attracted to the surface. It has been demonstrated for the same OPAG/IL mixture that such an electro-diffusion process is indeed controlled by the surface charge (Hjalmarsson et al., under review). Thermomechanical stresses cause the anions to decompose and it is thought that decomposition starts with the cleavage of a B-O bond, which simulations demonstrate to be energetically most vulnerable (Golets et al., 2016). Boron may contribute to formation of B2O3 and BPO4 while phosphorus may contribute to formation of phosphates and polyphosphates (Sharma et al., 2016). These compounds are known to provide wear resistant boundary films (McFadden et al., 1997; Shah et al., 2013). Compared to the case of borate ester addition to the IL/oil blend (Sharma et al., 2016), the use of orthoborate anions provides more boron in the boundary films enhancing the anti-wear performance. FIB-EDS was used to probe the thickness and composition of the selected patches, particularly since interfacially bound, unreacted IL might contribute to the EDS spectra in Figures 7, 8.

Figure 9 shows results for the ME/IL blend. The boron containing patch is rather wide and thick. Judging by the peak intensity, the boron content is much higher than the phosphorus content. A cross sectional cut of the patch reveals a uniform structure of up to 1,600 nm in thickness, probably composed largely of iron oxides, B2O3 and HBO2-III (Sharma et al., 2016; Spadaro et al., 2018). Similar observations can be made for the patches formed by the OPAG/IL blend. Figure 10 illustrates that the patch is once again enriched in boron with a smaller amount of phosphorus. Furthermore, the cross section of the patch reveals a homogeneous structure which is similar to, but much thinner than (800 nm), that formed by the ME/IL blend. This agrees well with the boron consumption trends revealed by the 11B NMR results. Hence, it can be concluded that the protective boundary films are similar in nature regardless of the base oil in which the IL was dissolved.

FIGURE 9
www.frontiersin.org

Figure 9. EDS spectra for points 1 (in black) and 2 (in red) and the corresponding FIB cross sectional cut of a patch formed on the surface lubricated by the ME/IL blend.

FIGURE 10
www.frontiersin.org

Figure 10. EDS spectrum for point 1 in the FIB cross sectional cut of a patch formed on the surface lubricated by the OPAG/IL blend.

Conclusion

The choice of IL as “next generation additive” to polar oils appears to be well-justified. It is clear that this non-halogenated IL forms stable, wear-reducing, boundary films in polar biodegradable oils. Importantly, it is the bis(mandelato)borate anion, rather than (as generally assumed) the tetraalkylphosphonium cation, which appears to answer for the majority of the composition of the boundary film.

The wear reduction is dramatic compared to the unformulated base oils in both cases, but there is a very strong dependence on the oil type, at least at the single, relevant temperature used here. The monoester performs better as a lubricant than the polyalkylglycol in the absence of IL, but this behavior is essentially reversed when IL is used as additive. In both cases reactions occur and wear films are formed but the wear film is much thinner in the polyalkylglycol than in the monoester and much less IL is consumed.

The study shows that the fields of chemistry and tribology are inextricably linked and provides a clear path forward for the chemical design of IL based anti-wear additives in synergy with the biodegradable oil. The choice of anion is as important as that of the cation and should be matched to both the cation and the oil.

Author Contributions

PR and BM performed and analyzed experiments. SG, OA, IF, and MR conceived the project. All authors contributed to the interpretation and writing of the manuscript.

Conflict of Interest Statement

The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Acknowledgments

The Knut and Alice Wallenberg Foundation (project No. KAW2012.0078) and the Swedish Research Council (project No. 2014-4694) are gratefully acknowledged for financial support.

Supplementary Material

The Supplementary Material for this article can be found online at: https://www.frontiersin.org/articles/10.3389/fchem.2019.00098/full#supplementary-material

References

Acharya, B., Avva, K. S., Thapa, B., Pardue, T. P., and Krim, J. (2018). Synergistic effect of nanodiamond and phosphate ester anti-wear additive blends. Lubricants 18:56. doi: 10.3390/lubricants6020056

CrossRef Full Text | Google Scholar

Archard, J. F. (1953). Contact and rubbing of flat surfaces. J. Appl. Phys. 24, 981–988. doi: 10.1063/1.1721448

CrossRef Full Text | Google Scholar

Chen, C., Bosse, H., and Deters, L. (2009). Effects of various base oils and additives on the tribological behaviour of lubricated aluminium- on-aluminium and steel-on-aluminium contacts. Proc. Inst. Mech. Eng. J. 223, 571–580. doi: 10.1243/13506501JET511

CrossRef Full Text | Google Scholar

Choi, U. S., Ahn, B. G., Kwon, O. K., and Chun, Y. J. (1997). Tribological behavior of some antiwear additives in vegetable oils. Tribol. Int. 30, 677–683. doi: 10.1016/S0301-679X(97)00039-X

CrossRef Full Text | Google Scholar

Cooper, P. K., Li, H., Rutland, M. W., Webber, G. B., and Atkin, R. (2016). Tribotronic control of friction in oil-based lubricants with ionic liquid additives. Phys. Chemist. Chem. Phys. 18, 23657–23662. doi: 10.1039/C6CP04405K

PubMed Abstract | CrossRef Full Text | Google Scholar

Cooper, P. K., Wear, C. J., Li, H., and Atkin, R. (2017). Ionic liquid lubrication of stainless steel: friction is inversely correlated with interfacial liquid nanostructure. ACS Sust. Chem. Eng. 5, 11737–11743. doi: 10.1021/acssuschemeng.7b03262

CrossRef Full Text | Google Scholar

Cowie, S., Cooper, P. K., Atkin, R., and Li, H. (2017). Nanotribology of ionic liquids as lubricant additives for alumina surfaces. J. Phys. Chem. C 121, 28348–28353. doi: 10.1021/acs.jpcc.7b09879

CrossRef Full Text | Google Scholar

Fujita, H., and Spikes, H. A. (2004). The formation of zinc dithiophosphate antiwear films. Proc. Instit. Mech. Eng. J. 218, 265–277. doi: 10.1243/1350650041762677

CrossRef Full Text | Google Scholar

Garcia, A., Gonzalez, R., Battez, A. H., Viesca, J. L., Monge, R., Fernandez-Gonzalez, A., et al. (2014). Ionic liquids as a neat lubricant applied to steel-steel contacts. Tribol. Int. 72, 42–50. doi: 10.1016/j.triboint.2013.12.007

CrossRef Full Text | Google Scholar

Glavatskih, S., and Höglund, E. (2008). Tribotronics: towards active tribology. Tribol. Int. 41, 934–939. doi: 10.1016/j.triboint.2007.03.001

CrossRef Full Text | Google Scholar

Goldstein, D. A., Mcguigan, M. A., and Ripley, B. D. (1988). Acute tricresylphosphate intoxication in childhood. Human Exp. Toxicol. 7, 179–182. doi: 10.1177/096032718800700213

PubMed Abstract | CrossRef Full Text | Google Scholar

Golets, M., Shimpi, M. R., Wang, Y. L., Antzutkin, O. N., Glavatskih, S., and Laaksonen, A. (2016). Understanding the thermal decomposition mechanism of a halogen-free chelated orthoborate-based ionic liquid: a combined computational and experimental study. Phys. Chem. Chem. Phys. 18, 22458–22466. doi: 10.1039/C6CP03191A

PubMed Abstract | CrossRef Full Text | Google Scholar

Jessop, P. G. (2018). Fundamental properties and practical applications of ionic liquids: concluding remarks. Faraday Discuss. 206, 587–601. doi: 10.1039/C7FD90090B

PubMed Abstract | CrossRef Full Text | Google Scholar

Johnson, D., and Hils, J. (2013). Phosphate esters, thiophosphate esters and metal thiophosphates as lubricant additives. Lubricants 18, 132–148. doi: 10.3390/lubricants1040132

CrossRef Full Text | Google Scholar

Kondo, Y., Yagi, S., Koyama, T., Tsuboi, R., and Sasaki, S. (2012). Lubricity and corrosiveness of ionic liquids for steel-on-steel sliding contacts. Proc. Instit. Mech. Eng. J. 226, 991–1006. doi: 10.1177/1350650112456127

CrossRef Full Text | Google Scholar

Kronberger, M., Pagano, F., Pejakovic, V., Igartua, A., Urbistondo, E., and Kalin, M. (2014). Miscibility and tribological investigations of ionic liquids in biodegradable esters. Lubricat. Sci. 26, 463–487. doi: 10.1002/ls.1274

CrossRef Full Text | Google Scholar

Kronberger, M., Pejakovic, V., Gabler, C., and Kalin, M. (2012). How anion and cation species influence the tribology of a green lubricant based on ionic liquids. Proc. Instit. Mech. Eng. J. 226, 933–951. doi: 10.1177/1350650112459012

CrossRef Full Text | Google Scholar

Li, H., Somers, A. E., Rutland, M. W., Howlett, P. C., and Atkin, R. (2016). Combined nano- and macrotribology studies of titania lubrication using the oil-ionic liquid mixtures. ACS Sust. Chem. Eng. 4, 5005–5012. doi: 10.1021/acssuschemeng.6b01383

CrossRef Full Text | Google Scholar

Mahipal, D., Krishnanunni, P., Mohammed Rafeekh, P., and Jayadas, N. H. (2014). Analysis of lubrication properties of zinc-dialkyl-dithio-phosphate (ZDDP) additive on Karanja oil (Pongamia pinnatta) as a green lubricant. Int. J. Eng. Res. 3, 494–496. doi: 10.17950/ijer/v3s8/804

CrossRef Full Text | Google Scholar

Martin, J. M. (1999). Antiwear mechanisms of zinc dithiophosphate: a chemical hardness approach. Tribol. Lett. 6, 1–8. doi: 10.1023/A:1019191019134

CrossRef Full Text | Google Scholar

McFadden, C., Soto, C., and Spencer, N. D. (1997). Adsorption and surface chemistry in tribology. Tribol. Int. 30, 881–888. doi: 10.1016/S0301-679X(97)00075-3

CrossRef Full Text | Google Scholar

Michaelis, S. (2011). Contaminated aircraft cabin air. J. Biol. Phys. Chem, 11, 132–145. doi: 10.4024/41111/11-4-abs1.jbpc.11.04

CrossRef Full Text | Google Scholar

Nakayama, K., Suzuki, N., and Hashimoto, H. (1992). Triboemission of charged particles and photons from solid surfaces during frictional damage. J. Phys. D Appl. Phys. 25, 303–308. doi: 10.1088/0022-3727/25/2/027

CrossRef Full Text | Google Scholar

Pejakovic, V., Kronberger, M., Mahrova, M., Vilas, M., Tojo, E., and Kalin, M. (2012). Pyrrolidinium sulfate and ammonium sulfate ionic liquids as lubricant additives for steel/steel contact lubrication. Proc. Instit. Mech. Eng. J 226, 923–932. doi: 10.1177/1350650112448978

CrossRef Full Text | Google Scholar

Qu, J., Barnhill, W. C., Luo, H., Meyer, H. M., Leonard, D. N., Landauer, A. K., et al. (2015). Synergistic effects between phosphonium-alkylphosphate ionic liquids and zinc dialkyldithiophosphate (ZDDP) as lubricant additives. Adv. Mater. 27, 4767–4774. doi: 10.1002/adma.201502037

PubMed Abstract | CrossRef Full Text | Google Scholar

Ramsden, J. J. (2013). On the proportion of ortho isomers in the tricresyl phosphates contained in jet oil. J. Biol. Phys. Chem 13, 69–72. doi: 10.4024/03RA13L.jbpc.13.02

CrossRef Full Text | Google Scholar

Shah, F. U., Glavatskih, S., and Antzutkin, O. N. (2013). Boron in tribology: from borates to ionic liquids. Tribol. Lett. 51, 281–301. doi: 10.1007/s11249-013-0181-3

CrossRef Full Text | Google Scholar

Shah, F. U., Glavatskih, S., Macfarlane, D. R., Somers, A., Forsyth, M., and Antzutkin, O. N. (2011). Novel halogen-free chelated orthoborate-phosphonium ionic liquids: synthesis and tribophysical properties. Phys. Chem. Chem. Phys. 13, 12865–12873. doi: 10.1039/c1cp21139k

PubMed Abstract | CrossRef Full Text | Google Scholar

Shahnazar, S., Bagheri, S., and Abd Hamid, S. B. (2016). Enhancing lubricant properties by nanoparticle additives. Int. J. Hydrogen Energy 41, 3153–3170. doi: 10.1016/j.ijhydene.2015.12.040

CrossRef Full Text | Google Scholar

Sharma, V., Doerr, N., Erdemir, A., and Aswath, P. B. (2016). Interaction of phosphonium ionic liquids with borate esters at tribological interfaces. RSC Adv. 6, 53148–53161. doi: 10.1039/C6RA11822D

CrossRef Full Text | Google Scholar

Spadaro, F., Rossi, A., Ramakrishna, S. N., Lainé, E., Woodward, P., and Spencer, N. D. (2018). Understanding complex tribofilms by means of H3BO3-B2O3 model glasses. Langmuir 34, 2219–2234. doi: 10.1021/acs.langmuir.7b01795

PubMed Abstract | CrossRef Full Text | Google Scholar

Spikes, H. (2015). Friction modifier additives. Tribol. Lett. 60:5. doi: 10.1007/s11249-015-0589-z

CrossRef Full Text | Google Scholar

Sweeney, J., Hausen, F., Hayes, R., Webber, G. B., Endres, F., Rutland, M. W., et al. (2012). Control of nanoscale friction on gold in an ionic liquid by a potential-dependent ionic lubricant layer. Phys. Rev. Lett. 109:155502. doi: 10.1103/PhysRevLett.109.155502

PubMed Abstract | CrossRef Full Text | Google Scholar

Totten, G. E., Shah, R. J., and Westbrook, S. R. (2003). Fuels and Lubricants Handbook: Technology, Properties, Performance, and Testing. Glen Bumie, MD: ASTM International.

Google Scholar

Westerholt, A., Weschta, M., Bösmann, A., Tremmel, S., Korth, Y., Wolf, M., et al. (2015). Halide-free synthesis and tribological performance of oil-miscible ammonium and phosphonium-based ionic liquids. ACS Sust. Chem. Eng. 3, 797–808. doi: 10.1021/sc500517n

CrossRef Full Text | Google Scholar

Xie, C., Toops, T. J., Lance, M. J., Qu, J., Viola, M. B., Lewis, S. A., et al. (2016). Impact of lubricant additives on the physicochemical properties and activity of three-way catalysts. Catalysts 6:54. doi: 10.3390/catal6040054

CrossRef Full Text | Google Scholar

Zhou, Y., and Qu, J. (2017). Ionic liquids as lubricant additives – a review. ACS Appl. Mater. Interfaces 9, 3209–3222. doi: 10.1021/acsami.6b12489

PubMed Abstract | CrossRef Full Text | Google Scholar

Keywords: biodegradable oil, ionic liquid, wear, friction, boundary lubrication, NMR

Citation: Rohlmann P, Munavirov B, Furó I, Antzutkin O, Rutland MW and Glavatskih S (2019) Non-halogenated Ionic Liquid Dramatically Enhances Tribological Performance of Biodegradable Oils. Front. Chem. 7:98. doi: 10.3389/fchem.2019.00098

Received: 08 November 2018; Accepted: 05 February 2019;
Published: 28 February 2019.

Edited by:

Jason B. Harper, University of New South Wales, Australia

Reviewed by:

Roberto D'Amato, Universidad Politécnica de Madrid (UPM), Spain
Alessandro Ruggiero, University of Salerno, Italy
Jacqueline Krim, North Carolina State University, United States

Copyright © 2019 Rohlmann, Munavirov, Furó, Antzutkin, Rutland and Glavatskih. This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.

*Correspondence: Mark William Rutland, bWFya0BrdGguc2U=

These authors have contributed equally to this work

Disclaimer: All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.